On this page
Galvannealed steel is sheet steel that is hot-dip galvanized and then immediately heated so iron from the base steel diffuses into the zinc, turning the coating into a zinc-iron alloy. The finished surface is matte gray with no spangle, and it is made specifically to be painted: it takes paint with excellent adhesion and spot welds more easily than regular galvanized sheet.
Galvannealed sheet is covered by ASTM A653, the same standard as galvanized, but it uses “A” coating designations instead of “G”. A40 and A60 are the two most commonly specified weights.
How galvannealed steel is made
Galvannealing happens on a continuous hot-dip line. The steel strip is cleaned, annealed and passed through a molten zinc bath, and air knives wipe the coating to the target weight, just as for galvanized sheet. The difference comes next: instead of cooling, the strip runs straight into a galvannealing furnace that holds it hot for a short time.
During that heat cycle, iron and zinc diffuse into each other. The soft, bright zinc layer is converted completely into a series of harder zinc-iron intermetallic phases, with a typical iron content of roughly 8 to 12% in the finished coating. Bath chemistry, line speed and furnace temperature are controlled tightly, because too little alloying leaves free zinc on the surface and too much makes the coating brittle.
The resulting surface has a fine, slightly rough texture at a microscopic level. That texture, plus the absence of free zinc that can react with some paint binders, is what makes galvanneal such a good paint base.
A40 and A60 coating weights
ASTM A653 measures galvannealed coatings the same way as galvanized: the number is the minimum total coating on both sides in hundredths of an ounce per square foot, by the triple spot test.
| Designation | Min total, triple spot | Min one side, triple spot | Min total, single spot |
|---|---|---|---|
| A25 | 0.25 oz/ft² | 0.08 oz/ft² | 0.20 oz/ft² |
| A40 | 0.40 oz/ft² | 0.12 oz/ft² | 0.30 oz/ft² |
| A60 | 0.60 oz/ft² | 0.20 oz/ft² | 0.50 oz/ft² |
A01 also exists and carries no minimum. In metric units, A40 and A60 correspond roughly to ZF120 and ZF180 (about 120 and 180 g/m² total). Because the zinc-iron alloy has a density close to zinc, the thickness is similar to galvanized sheet of the same weight: about 0.34 mil (9 µm) per side for A40 and about 0.51 mil (13 µm) per side for A60.
Galvannealed coatings are rarely made heavier than A60. Thick zinc-iron layers become brittle and tend to crack and flake during forming, which is why galvanneal is produced as a light to moderate coating designed to work under paint.
Choosing A40 or A60
- A40 suits painted parts for interior service: cabinets, panels, lockers and appliance components where the paint film does most of the work.
- A60 is the usual choice when painted parts face humidity, temperature swings or exterior exposure. Hollow metal door and frame standards, for example, commonly call for A60 (or G60) on exterior openings.
Tip: A40 and G40, or A60 and G60, carry the same minimum coating weight but are different products. Galvannealed is chosen for paint and welding; galvanized for bare corrosion protection. Write the letter on the order.
Why fabricators choose galvanneal
Paint adhesion
Fresh galvanized zinc is smooth and chemically active, so paint can lose adhesion unless the surface is carefully prepared. Galvanneal’s alloyed surface accepts phosphate pretreatments and primers readily, so paint and powder coat systems bond well. The surface also has no spangle pattern to telegraph through a thin paint film, which helps on visible appliance and enclosure panels.
Spot welding
Pure zinc melts at a low temperature and alloys aggressively with copper welding electrodes, which shortens electrode life on galvanized sheet. The zinc-iron coating on galvanneal has a higher melting point and reacts less with the copper, so resistance spot welds form more consistently and electrodes last longer between dressings. That is a major reason galvanneal has long been used for automotive body panels and other high-volume welded sheet assemblies.
Corrosion protection under paint
Galvanneal still protects the steel galvanically. When paint is scratched or chipped, the zinc in the coating slows rust creep under the film, so painted galvanneal resists undercutting far better than painted bare steel. That combination of paint and zinc is why it is common on cabinets and doors that see condensation, cleaning or weather after installation.
Limitations to plan around
- Powdering in severe forming: the alloy coating is harder and less ductile than zinc. In tight bends, hems and deep draws it can crack and shed fine particles, called powdering. Use generous bend radii, good lubrication, and Forming Steel (FS) or Drawing Steel grades where forming is severe.
- Appearance when bare: unpainted galvanneal is dull and can weather to an uneven, slightly reddish tone as the iron in the coating oxidizes. It is made to be painted.
- Light coatings only: because coatings top out around A60, parts that need heavy bare corrosion protection should use G90 galvanized steel or heavier.
- Arc welding fumes: like any zinc coating, galvanneal releases zinc oxide fume when arc welded, so fume extraction is required.
Common uses of galvannealed steel
- Hollow metal doors, frames and other painted architectural openings
- Electrical enclosures, control cabinets and junction boxes
- Appliance cabinets and panels, washer and dryer housings
- Office furniture, lockers, shelving and storage cabinets
- HVAC equipment cabinets that are painted at the factory
- Signage, kiosks and vending machine housings
- Painted enclosures and racking for energy storage and electrical equipment
The common thread is a painted, often spot welded part where appearance and paint durability matter. For a side-by-side with the other coated sheet products, see galvanized vs galvannealed vs Galvalume.
Ordering galvannealed sheet
A galvanneal callout follows the same pattern as galvanized: specification, base steel designation, coating, surface condition and thickness. For example: ASTM A653 CS Type B, A60, dry, 16 gauge (0.0635 in). Commercial Steel suits most bent panels and cabinets; Forming Steel helps where hems and tight flanges are common. Ask for oiled or dry material depending on how the parts will be cleaned and pretreated, and tell the supplier the sheet will be painted so any surface treatment does not interfere with the finish.
Galvannealed sheet is ordered by the same gauge decimals as galvanized, so the sheet metal gauge chart for coated sheet applies.
Galvannealed steel from ASA
ASA’s stock list includes galvannealed sheet in A40 and A60 to ASTM A653, alongside galvanized, Galvalume and aluminized steel in its flat-rolled sheet and plate line. Mill certifications and full material traceability are available. ASA can level and cut coated sheet to length, laser cut, press brake form, weld and powder coat galvannealed parts in house, with most JIT orders delivered in 24 to 48 hours.
Frequently asked questions
Is galvannealed steel the same as galvanized?
Both start with a hot-dip zinc coating on sheet steel under ASTM A653, but galvannealed sheet is reheated right after coating so the zinc alloys with iron. That changes the surface from bright, spangled zinc to a matte gray zinc-iron alloy. Galvanized is chosen for bare corrosion resistance; galvannealed is chosen for painted and spot welded parts.
Can galvannealed steel be left unpainted?
It can survive indoors without paint, but it is not designed for it. Bare galvanneal looks dull and can take on an uneven reddish tint as the iron in its coating weathers, and its coatings are lighter than most galvanized grades used bare. For unpainted parts, galvanized sheet in G60 or G90 usually gives better appearance and longer protection.
What does A60 mean on a galvannealed sheet?
A60 means the zinc-iron coating weighs at least 0.60 ounces per square foot of sheet, both sides combined, averaged over three samples by the triple spot test. Any single sample must reach 0.50 oz/ft² and each side 0.20 oz/ft². The letter A identifies galvannealed coating under ASTM A653, as opposed to G for galvanized.
Why does galvannealed coating flake when bent?
The zinc-iron intermetallic phases that form during galvannealing are harder and less ductile than pure zinc. Tight bends, hems and draws put the coating in compression on the inside of the bend, where it can crack and shed fine particles. This is called powdering. Larger bend radii, lubrication and forming grades of steel reduce it.
Is galvannealed steel good for powder coating?
Yes. Galvanneal is one of the preferred substrates for powder coating because its alloyed, slightly textured surface bonds well with pretreatments and powder. It also tends to give a smoother finish than spangled galvanized sheet. Parts still need proper cleaning before coating, and the finisher should know the substrate so cure and pretreatment settings suit it.