G90 Galvanized Steel: Coating Weight, Specs and Uses

G90 galvanized steel carries at least 0.90 oz/ft² of zinc across both sides. Here is what that means, how it compares with G60, and how to order it.

Updated October 2026 5 min read By the ASA team

On this page
  1. What the G90 designation means
  2. G60 vs G90 galvanized
  3. ASTM A653 steel designations: CS, FS and SS
  4. G90 galvanized gauge thicknesses
  5. Common uses of G90 galvanized steel
  6. Buying G90 galvanized from ASA

G90 galvanized steel is hot-dip galvanized sheet with a minimum of 0.90 oz/ft² (about 275 g/m²) of zinc, measured as the total on both sides by the ASTM A653 triple spot test. That works out to roughly 0.76 mil (19 µm) of zinc per side, which makes G90 the standard choice for outdoor, humid and moderately corrosive service.

This page covers what the G90 designation guarantees, how it compares with G60, which A653 steel designations to order, and where G90 is typically used. For background on how galvanizing works, see what is galvanized steel.

What the G90 designation means

In ASTM A653, the number after the “G” is the minimum total zinc coating weight on both surfaces, in hundredths of an ounce per square foot of sheet. G90 sheet must meet two minimums:

RequirementG90 minimum
Triple spot test (average of 3 samples), total both sides0.90 oz/ft² (275 g/m²)
Single spot test (any one sample), total both sides0.80 oz/ft² (244 g/m²)
Approximate coating per side, at the triple spot minimum with an even split0.45 oz/ft², about 0.76 mil (19 µm)

The triple spot test takes samples from the center and both edges of the sheet width and averages them. The single spot test is the floor for any one of those samples. A653 also sets a triple spot minimum for each side, 0.32 oz/ft² for G90, so one face cannot carry nearly all of the coating.

A common mistake is to read G90 as 0.90 oz/ft² per side. It is the total. If a drawing or specification calls for a per side thickness in mils or microns, convert it before ordering: 1 oz/ft² of zinc is about 1.7 mils (43 µm) thick.

Tip: The metric equivalent of G90 is Z275, the total coating mass in grams per square meter. Specifications written to European or international standards often call for Z275 where a US drawing would say G90.

G60 vs G90 galvanized

G60 and G90 are the two most widely specified coating weights. G90 carries 50% more zinc than G60, and because zinc is consumed gradually, its time to first rust in the same environment is roughly 50% longer.

PropertyG60G90
Min total coating, triple spot0.60 oz/ft² (183 g/m²)0.90 oz/ft² (275 g/m²)
Min total coating, single spot0.50 oz/ft²0.80 oz/ft²
Approx thickness per side0.51 mil (13 µm)0.76 mil (19 µm)
Typical exposureIndoor, dry or protectedOutdoor, humid, washdown
Metric equivalentAbout Z180About Z275

G60 is common for indoor ductwork, interior framing and appliance parts where the coating mainly guards against handling and humidity. G90 costs slightly more and is the safer choice when parts will see weather, condensation or periodic washdown. For severe industrial or coastal exposure, heavier coatings such as G115 or above, a paint over galvanizing (duplex) system, or a different material may be the better fit.

ASTM A653 steel designations: CS, FS and SS

The coating weight is only half of a G90 order. ASTM A653 also defines the base steel, and the designation controls how the sheet will behave in forming and what strength you can design to.

DesignationNameUse
CS (Types A, B, C)Commercial SteelGeneral bending and moderate forming; no guaranteed strength
FS (Types A, B)Forming SteelMore severe forming and roll forming
DDS, EDDSDeep Drawing and Extra Deep Drawing SteelDrawn parts with severe stretching
SS (Grades 33 to 80)Structural SteelLoad bearing parts with specified minimum yield and tensile
HSLASHigh Strength Low Alloy SteelHigher strength with better formability than SS at the same yield

CS Type B is the most common default for general fabrication. When the part carries load and the design relies on a minimum yield, order SS with a grade. Common examples:

A653 SS gradeMin yieldMin tensile
Grade 3333 ksi (230 MPa)45 ksi (310 MPa)
Grade 4040 ksi (275 MPa)55 ksi (380 MPa)
Grade 50 Class 150 ksi (340 MPa)65 ksi (450 MPa)

A complete callout names the specification, designation, grade if any, coating and thickness, for example: ASTM A653 SS Grade 33, G90, 16 gauge (0.0635 in).

G90 galvanized gauge thicknesses

Galvanized sheet uses its own gauge table. The decimal thickness includes the coating and runs slightly heavier than the same gauge number in uncoated steel. The full comparison is in the sheet metal gauge chart.

GaugeNominal thicknessNominal weight
100.1382 in (3.51 mm)5.781 lb/ft²
110.1233 in (3.13 mm)5.156 lb/ft²
120.1084 in (2.75 mm)4.531 lb/ft²
140.0785 in (1.99 mm)3.281 lb/ft²
160.0635 in (1.61 mm)2.656 lb/ft²
180.0516 in (1.31 mm)2.156 lb/ft²
200.0396 in (1.01 mm)1.656 lb/ft²
220.0336 in (0.85 mm)1.406 lb/ft²
240.0276 in (0.70 mm)1.156 lb/ft²
260.0217 in (0.55 mm)0.906 lb/ft²

Common uses of G90 galvanized steel

  • HVAC: ductwork, plenums, rooftop unit housings and curbs, especially in exterior, humid or unconditioned spaces.
  • Outdoor enclosures: electrical, telecom and controls cabinets, and battery energy storage enclosures, often with powder coat over the zinc.
  • Framing: light gauge studs, tracks, joists and purlins. Framing standards commonly set G60 as a minimum for structural members, and G90 is often specified for exterior walls and humid or coastal sites.
  • Building products: roofing, siding, flashing, gutters and trim.
  • Equipment: agricultural equipment, panels, guards and covers that live outdoors.
  • Data center hardware: cable trays, brackets and containment components where a durable, low maintenance finish is needed.

G90 is formable enough for press brake bending and roll forming, and it can be laser cut, punched and sheared. Cut edges are protected for a time by the surrounding zinc, which is one reason galvanized sheet works well for fabricated parts.

Handling and fabrication notes

Store G90 bundles dry and under cover. Moisture trapped between tightly stacked sheets causes white rust (wet storage stain), which dulls the surface and, if left long enough, consumes coating.

When G90 parts are welded, the zinc burns off near the joint. Use fume extraction, and restore protection on the heated area with zinc rich paint. For assemblies that need full coverage over welds and cut edges, batch hot-dip galvanizing after fabrication to ASTM A123 is the alternative to building from pre-galvanized sheet.

Buying G90 galvanized from ASA

American Steel & Aluminum stocks ASTM A653 galvanized sheet, mainly in G90, in its flat-rolled sheet and plate line, with mill certifications and full material traceability available. ASA’s leveling and cut-to-length line processes coated steel from 24 to 11 gauge, and parts can be laser cut, press brake formed, welded and powder coated in house. ASA’s company-owned trucks serve New England and New York, and JIT delivery gets most orders to customers in 24 to 48 hours.

Frequently asked questions

Is G90 galvanized good for outdoor use?

Yes. G90 is the most common coating weight specified for outdoor sheet metal in typical rural, suburban and light industrial settings. Its zinc layer protects the steel for many years before red rust appears. In harsh coastal or chemical environments, consider a heavier coating, a paint or powder coat over the zinc, or a different material such as stainless or aluminum.

How thick is the zinc on G90 galvanized steel?

At the 0.90 oz/ft² triple spot minimum, the total zinc is about 1.53 mils (39 µm), split between the two surfaces. That means each side carries roughly 0.76 mil (19 µm). Actual coatings are often slightly heavier than the minimum. The zinc thickness is part of the nominal gauge thickness of galvanized sheet, not added on top of it.

Can G90 galvanized steel be painted or powder coated?

Yes, with proper surface preparation. Mill passivation treatments and oils on new galvanized sheet can cause poor adhesion, so parts are cleaned and pretreated before coating. Powder coaters also watch for outgassing from the zinc during cure, which can leave pinholes in the finish. A paint or powder system over G90 extends service life well beyond either protection alone.

Will G90 galvanized steel rust at cut edges?

Usually not right away. When sheet is sheared, punched or laser cut, the exposed steel edge is protected by the surrounding zinc, which corrodes sacrificially in its place. On thin gauges in normal outdoor exposure this protection works well. On thicker material or in wet, salty conditions, edges may show rust sooner and benefit from touch up paint or a powder coat.

What is the difference between G90 and Z275?

They describe nearly the same coating in different units. G90 is the US designation from ASTM A653, meaning at least 0.90 ounces of zinc per square foot total on both sides. Z275 is the metric designation for 275 grams per square meter total. Because the test methods and tolerances differ slightly, confirm which standard governs the order.

Material, processing and fabrication from one supplier