ASTM A653: Galvanized Steel Sheet Specification

How ASTM A653 coating designations and steel designations work together, the surface options it allows, and how to write a complete galvanized order.

Updated October 2026 5 min read By the ASA team

On this page
  1. What ASTM A653 covers
  2. Coating designations and what they guarantee
  3. Base steel designations and structural grades
  4. Surface options
  5. Thickness: coating included
  6. What to write on a purchase order
  7. Buying A653 sheet from ASA

ASTM A653 is the standard specification for steel sheet that is zinc-coated (galvanized) or zinc-iron alloy-coated (galvannealed) by the continuous hot-dip process, in coils and cut lengths. Every A653 order needs two things: a coating designation such as G60, G90 or A40, which sets the minimum weight of zinc, and a steel designation such as CS Type B or SS Grade 33, which sets the base metal chemistry and, for structural grades, its strength.

A653 relies on ASTM A924, the general requirements specification for hot-dip metallic-coated sheet, for tolerances, sampling and test procedures. This guide covers how the coating and steel designations work, the surface options and the thickness rules that trip up many orders.

What ASTM A653 covers

A653 covers sheet coated on a continuous line, where cleaned and annealed steel strip runs through molten zinc and the coating is wiped to a controlled weight. The bath must contain at least 99% zinc, with a small aluminum addition that limits the brittle zinc-iron layer and helps the coating adhere. Parts galvanized after fabrication in a kettle are a different product under ASTM A123, covered in the guide to galvanized steel.

Two coating types are covered. “G” designations are galvanized: essentially pure zinc, bright, with or without visible spangle. “A” designations are galvannealed: the zinc is heat treated right after coating so iron diffuses through it, leaving a matte gray zinc-iron alloy that paints and spot welds well. Metric orders under A653M use Z and ZF designations in grams per square meter.

Coating designations and what they guarantee

The number in a coating designation is the minimum triple spot average, total of both sides, in hundredths of an ounce per square foot. G90 therefore means at least 0.90 oz/ft² of zinc across both faces, not on each face.

DesignationTriple spot, total both sidesTriple spot, one sideSingle spot, total both sidesMetric designation
G300.300.100.25Z90
G400.400.120.30Z120
G600.600.200.50Z180
G900.900.320.80Z275
G1151.150.401.00Z350
A250.250.080.20ZF75
A400.400.120.30ZF120
A600.600.200.50ZF180

All values are in oz/ft² from the A653 coating table. The triple spot test averages samples taken from the edge, center and other edge of the full-width sheet; the single spot test is the minimum any one sample may show. The one-side column is the minimum triple spot weight on each face, which limits how unevenly the coating can be split. Heavier designations, up to G360 in the standard, exist for severe exposure but are rarely available in thin gauges.

A653 gives a conversion for estimating thickness: 1 oz/ft² of coating is about 1.7 mils. With an even split at the triple spot minimum, that works out to about 0.51 mil (13 µm) per side for G60 and about 0.76 mil (19 µm) per side for G90. For a side-by-side look at the zinc-iron option, see galvannealed steel.

Tip: The triple spot requirement applies to the original full-width sheet. Narrow material slit from it is checked against the single spot minimum, so a G90 slit coil can test below 0.90 oz/ft² at a single location and still conform.

Base steel designations and structural grades

DesignationNameDefault when type not given
CS Types A, B, CCommercial SteelType B
FS Types A, BForming SteelType B
DDS Types A, CDeep Drawing SteelType A
EDDSExtra Deep Drawing SteelNot applicable
SSStructural Steel (by grade and class)Grade must be stated
HSLAS, HSLAS-FHigh-Strength Low-Alloy Steel, and with Improved FormabilityGrade must be stated
SHS, BHSSolution Hardened and Bake Hardenable SteelGrade must be stated

For CS, FS, DDS and EDDS, A653 controls chemistry and gives only typical, nonmandatory mechanical properties. CS Type B (carbon 0.02 to 0.15%) is the common choice for general fabrication; FS is for more severe forming and roll forming; DDS and EDDS are for deep drawing. When a design depends on strength, order a structural or high-strength designation, which carries tested minimums on the base metal:

SS gradeYield, minTensile, minElongation in 2 in, min
3333 ksi (230 MPa)45 ksi (310 MPa)20%
3737 ksi (255 MPa)52 ksi (360 MPa)18%
4040 ksi (275 MPa)55 ksi (380 MPa)16%
50 Class 150 ksi (340 MPa)65 ksi (450 MPa)12%
50 Class 350 ksi (340 MPa)70 ksi (480 MPa)12%
50 Class 450 ksi (340 MPa)60 ksi (410 MPa)12%
8080 ksi (550 MPa)82 ksi (570 MPa)No requirement

SS Grade 50 comes in classes that differ by tensile strength (Class 2 has no tensile minimum), and Grade 80 is a full hard product with no elongation requirement. The values here follow the A653/A653M-05 tables. Recent editions have revised and added designations, so cite the edition on the order and check its tables.

Surface options

  • Spangle. Regular spangle shows the visible zinc crystal pattern. Minimized spangle has a smaller, less distinct pattern and is normally produced in G90 and lighter. Spangle-free shows no visible pattern and suits painted parts.
  • Chemical treatment. Most galvanized sheet is chemically treated (passivated) to resist white rust in storage. Treated sheet may need extra cleaning or pretreatment before paint or powder coat, so order “not chemically treated” when parts will be coated, and store that sheet dry.
  • Oiled or not oiled. Oil also helps against storage stain but must be removed before coating or welding.
  • Phosphatized and extra smooth. Optional treatments for paint adhesion and for a smoother surface on painted panels.

Galvanized G coatings on most steel designations must pass a 180 degree coating bend test without flaking (some higher strength grades, such as SS Grades 50 and 80, are exempt). Galvannealed A coatings are exempt because the zinc-iron alloy is less ductile and can powder in severe forming, which is worth knowing before specifying galvannealed for tight bends.

Thickness: coating included

Under A653, ordered thickness includes both the base steel and the coating, expressed to 0.001 in (0.01 mm), as a minimum or a nominal. The buyer also chooses which A924 thickness tolerance table applies, the one measured 3/8 in from the edge or the one measured 1 in from the edge. If a design needs a guaranteed base metal thickness, A653 has a supplementary requirement for ordering to base metal thickness instead.

Galvanized gauge numbers already include an allowance for zinc, so 16 gauge galvanized is 0.0635 in against 0.0598 in for bare steel. Order by decimal to avoid confusion.

What to write on a purchase order

  • Product name: steel sheet, zinc-coated (galvanized) or zinc-iron alloy-coated (galvannealed)
  • ASTM A653 (or A653M) and year of issue
  • Steel designation, with type, grade and class as applicable
  • Coating designation
  • Chemically treated or not, oiled or not, minimized spangle or extra smooth if required
  • Thickness (minimum or nominal) and tolerance table, width, and length or coil size
  • Certification, application and quantity

Example: Steel sheet, zinc-coated, ASTM A653-XX, SS Grade 33, coating G90, not chemically treated, oiled, 0.064 nominal x 48 x 120 in, mill test report required, for outdoor enclosure.

Buying A653 sheet from ASA

American Steel & Aluminum stocks galvanized sheet, mainly in G90, and galvannealed in A40 and A60, with ASTM A653 on its stock list. Coated sheet from 24 to 11 gauge can be leveled and cut to length, then laser cut, formed and welded in-house. Request a quote with both the steel and coating designation.

Frequently asked questions

Does ASTM A653 thickness include the zinc coating?

Yes. Unless the order invokes the supplementary requirement for base metal thickness, A653 thickness is measured over the coating, so it includes both the steel and the zinc. The order states it as a minimum or nominal value, along with the A924 tolerance table that applies. Heavy coatings therefore leave slightly less steel at the same ordered thickness.

What is the difference between ASTM A653 and ASTM A123?

A653 covers sheet coated on a continuous line before fabrication, sold by coating designations such as G60 and G90. A123 covers parts, shapes and assemblies dipped in a zinc kettle after fabrication, with minimum coating thickness set by steel category and thickness. A123 coatings are typically much heavier and cover welds and cut edges.

What is minimized spangle?

Spangle is the visible crystal pattern zinc forms as it solidifies. Minimized spangle is produced by controlling that solidification so the pattern is smaller and less distinct, which gives a more uniform surface for painting. A653 notes it is normally produced in coating designations G90 and lighter. It must be requested on the order.

Can galvannealed A653 sheet be bent?

Yes, within limits. Galvannealed sheet forms well in ordinary press brake work, but its zinc-iron coating is harder and less ductile than galvanized zinc, so very tight bends or severe draws can cause powdering, where flakes of coating break off. For that reason A653 does not apply its coating bend test to galvannealed designations.

Material, processing and fabrication from one supplier