  1. What ASTM A1011 covers
  2. Designations and chemistry
  3. Mechanical requirements by grade
  4. Surface condition, oiling and edges
  5. A1011 SS Grade 36 and A36
  6. What to write on a purchase order
  7. Buying A1011 sheet from ASA

ASTM A1011 is the standard specification for hot rolled carbon, structural, high-strength low-alloy and ultra-high strength steel sheet and strip, supplied in coils and cut lengths. It is the spec behind most hot rolled sheet bought in the US, from commercial quality (CS) used for brackets and frames to structural (SS) and HSLAS grades bought to a guaranteed yield strength.

A1011 stops at heavy-thickness coil, which is covered by ASTM A1018. This guide explains the A1011 designations, the strength each grade must meet, the surface and edge options, and how to write an order that gets you the material you expect. Values below are from the A1011/A1011M-09a edition; confirm them against the current edition or the edition named on your order.

What ASTM A1011 covers

A1011 is a product specification for hot rolled sheet and strip. General requirements come from two companion standards: ASTM A568 for sheet and ASTM A749 for strip. Those documents hold the thickness, width and flatness tolerance tables, the rules for retests and much of the testing detail, so an A1011 order effectively invokes them as well.

The mechanical property tables in A1011 run up to just under 0.230 in (6.0 mm) thick. Hot rolled coil from 0.230 to 1.000 in is a separate product under ASTM A1018, which exists because thick coil is processed and tested differently from discrete plate.

Several defaults apply when an order is silent. If no type is named for CS or DS, Type B is furnished. If no class is named for HSLAS, Class 1 is furnished. SS Grade 36 defaults to Type 1, and UHSS defaults to Type 1.

Designations and chemistry

DesignationWhat it isStrength valuesChoose it for
CS Types A, B, C, DCommercial SteelTypical onlyGeneral fabrication, brackets, frames, moderate bending
DS Types A, BDrawing SteelTypical onlyFormed and drawn parts that need more stretch
SS Grades 30 to 80Structural SteelMandatory minimumsParts designed to a minimum yield strength
HSLAS Classes 1 and 2, Grades 45 to 70High-Strength Low-Alloy SteelMandatory minimumsHigher strength, lighter sections
HSLAS-F Grades 50 to 80HSLAS with Improved FormabilityMandatory minimumsHigh strength parts with tight bends
UHSS Grades 90 and 100Ultra-High Strength SteelMandatory minimumsMaximum strength to weight in sheet

CS Type B, with carbon held between 0.02 and 0.15% and manganese at 0.60% maximum, is the workhorse designation for general hot rolled fabrication. The standard notes that CS Type B and DS Type B describe the most common products of the older commercial and drawing steel specifications, A569 and A622, both since withdrawn. CS Type D allows slightly more manganese (0.70% max) with carbon at 0.10% max.

For CS and DS, chemistry is mandatory and strength is not. The standard’s typical, nonmandatory values are 30 to 50 ksi (205 to 340 MPa) yield with at least 25% elongation for CS, and 30 to 45 ksi (205 to 310 MPa) yield with at least 28% elongation for DS, measured on material 0.100 to 0.150 in thick. Thinner sheet tends to be stronger and less ductile.

Structural grades allow up to 0.25% carbon, with manganese at 0.90% maximum for the lower grades and 1.35% for Grade 36 Type 2 and the stronger grades. HSLAS, HSLAS-F and UHSS add microalloying elements such as columbium (niobium), vanadium and titanium. See HSLA steel for how microalloying raises strength without adding carbon.

Mechanical requirements by grade

For SS, HSLAS, HSLAS-F and UHSS, the grade number is the minimum yield strength in ksi, and the mill must report both the heat analysis and the tension test results.

DesignationYield, minTensileElongation in 2 in, min*
SS Grade 3030 ksi (205 MPa)49 ksi (340 MPa) min25%
SS Grade 3333 ksi (230 MPa)52 ksi (360 MPa) min23%
SS Grade 36 Type 136 ksi (250 MPa)53 ksi (365 MPa) min22%
SS Grade 36 Type 236 ksi (250 MPa)58 to 80 ksi (400 to 550 MPa)21%
SS Grade 4040 ksi (275 MPa)55 ksi (380 MPa) min21%
SS Grade 5050 ksi (340 MPa)65 ksi (450 MPa) min17%
SS Grade 6060 ksi (410 MPa)75 ksi (520 MPa) min14%
HSLAS Grade 50, Class 150 ksi (340 MPa)65 ksi (450 MPa) min22%
HSLAS Grade 50, Class 250 ksi (340 MPa)60 ksi (410 MPa) min22%
HSLAS-F Grade 5050 ksi (340 MPa)60 ksi (410 MPa) min24%
UHSS Grade 9090 ksi (620 MPa)100 ksi (690 MPa) min16%

*Elongation requirements in A1011 depend on thickness. The values shown apply to sheet 0.097 in (2.5 mm) and thicker; thinner sheet has lower minimums. HSLAS Class 2 trades 5 ksi of minimum tensile strength and a lower carbon ceiling for better formability. The standard lists a full set of grades up to SS Grade 80, HSLAS Grade 70 and UHSS Grade 100.

Bend guidance

DesignationSuggested minimum inside bend radius (90 degree bend)
SS Grades 30 and 331 t
SS Grade 36 Type 11-1/2 t
SS Grade 36 Type 2 and Grade 402 t
SS Grade 502-1/2 t
HSLAS Grade 50, Class 1 / Class 22 t / 1-1/2 t
HSLAS-F Grade 501 t

These radii come from the standard’s nonmandatory appendix and assume good shop practice. A bend line parallel to the rolling direction is the harder way to bend, so orient bend lines across it where the nest allows, and consult the producer when a part needs a tighter radius than listed.

Surface condition, oiling and edges

Unless the order says otherwise, A1011 material is furnished as rolled, with the hot rolled oxide (mill scale) left on the surface, and not oiled. The order can instead call for pickled or blast cleaned material, which removes the scale; pickled or blast cleaned material is furnished oiled unless dry is specified. Pickled and oiled sheet, often written HRPO or P&O, is the usual choice for parts that will be painted, powder coated or welded without grinding.

Sheet and strip are both available with mill edge or cut edge. Mill edge is the rounded edge left by hot rolling and is fine for parts that will be blanked or laser cut inside the edge. Cut edge (slit or sheared) gives a square edge and an exact width.

The order should also name the thickness tolerance table from ASTM A568 or A749 that applies. Not every producer can meet every tolerance table, so tight thickness requirements belong in the inquiry, not just the purchase order.

Tip: Mill scale is hard on press brake tooling, interferes with paint adhesion and can contaminate welds. If parts will be coated or welded as cut, price pickled and oiled sheet against the cost of removing scale later.

A1011 SS Grade 36 and A36

Drawings often call for A36 on parts made from hot rolled sheet. Strictly, A36 steel is a specification for plate, shapes and bars. For sheet, A1011 SS Grade 36 Type 2 is the usual match: 36 ksi (250 MPa) minimum yield and a tensile range of 58 to 80 ksi (400 to 550 MPa), the same yield and tensile range A36 sets for plate up to 8 in thick. Type 1 has the same yield but only a 53 ksi minimum tensile, so name the type when the strength range matters.

What to write on a purchase order

  • ASTM A1011 (or A1011M) and year of issue
  • Hot rolled sheet or strip, designation, and type, grade or class
  • Finish: as rolled, pickled, or blast cleaned; oiled or dry
  • Edge: mill edge or cut edge
  • Thickness, applicable tolerance table, width, and cut length or coil (with ID, OD and maximum weight)
  • Copper bearing steel, if required
  • Quantity, part number or application, and certification required

Example: ASTM A1011-XX, hot rolled steel sheet, SS Grade 36 Type 2, pickled and oiled, cut edge, 0.1345 x 48 x 120 in, thickness tolerance per ASTM A568, mill test report required, for equipment base. Compare the cold rolled equivalent in ASTM A1008, which uses a similar structure but different defaults.

Buying A1011 sheet from ASA

American Steel & Aluminum stocks hot rolled carbon steel, and ASTM A1011 is on its stock list alongside HSLA and plain carbon chemistries. ASA can level and cut to length carbon sheet from 24 to 11 gauge, laser cut and form parts, and supply mill certifications with full traceability. Request a quote with the designation, finish and thickness you need.

Frequently asked questions

What does HRPO mean?

HRPO stands for hot rolled, pickled and oiled. The sheet is rolled hot, then run through an acid pickling line that removes mill scale, and finally coated with a light oil to slow rusting. Under ASTM A1011, an order must ask for pickled material, since the default is as rolled with scale and no oil.

Is A1011 SS Grade 36 the same as A36?

Not exactly. A36 covers plate, shapes and bars, while A1011 covers hot rolled sheet and strip. A1011 SS Grade 36 Type 2 matches A36 strength, 36 ksi minimum yield and 58 to 80 ksi tensile, and is the usual substitute when a drawing says A36 on a sheet part. Type 1 has a lower tensile minimum.

How thick can ASTM A1011 sheet be?

The A1011 mechanical property tables cover material up to just under 0.230 in (6.0 mm) thick. Hot rolled coil from 0.230 in through 1.000 in falls under ASTM A1018, the heavy-thickness coil specification. Thicker flat material is normally bought as discrete plate under specifications such as A36, with dimensional rules from ASTM A6.

What does Type B mean in ASTM A1011 commercial steel?

Type B is one of four chemistry options for commercial steel. It holds carbon between 0.02 and 0.15% with manganese at 0.60% maximum, which avoids the ultra-low carbon steels that Types A and C may include. It is the most common hot rolled commercial grade and is what the mill supplies when an order does not name a type.

Material, processing and fabrication from one supplier

Send a drawing or a material list and the ASA team will quote it from stock.