What Is Aluminized Steel? ASTM A463 Explained

Aluminized steel is carbon steel with a hot-dip aluminum coating: Type 1 resists heat and Type 2 resists weather. Learn how ASTM A463 defines each and where they are used.

Updated October 2026 5 min read By the ASA team

On this page
  1. Type 1 vs Type 2 aluminized steel
  2. ASTM A463 coating designations
  3. Heat resistance of aluminized steel
  4. Corrosion behavior and cut edges
  5. Fabricating aluminized steel
  6. Aluminized steel from ASA

Aluminized steel is carbon steel sheet hot-dip coated with aluminum or an aluminum-silicon alloy, made to ASTM A463. The coating gives the steel resistance to heat oxidation and atmospheric corrosion that plain or galvanized steel cannot match, at far lower cost than stainless steel.

There are two types. Type 1 carries an aluminum-silicon coating and is used mainly for heat resistance in exhaust, oven and furnace parts. Type 2 carries commercially pure aluminum and is used mainly for long-life outdoor corrosion resistance in roofing, siding and drainage products.

Type 1 vs Type 2 aluminized steel

FeatureType 1Type 2
CoatingAluminum with 5 to 11% siliconCommercially pure aluminum
Main strengthHeat and oxidation resistanceAtmospheric corrosion resistance
Common designationT1-40T2-65
FormabilityGood; thin alloy layerModerate; thicker coating
Typical usesExhaust, heat shields, ovens, furnacesRoofing, siding, drainage structures

Why silicon matters in Type 1

When steel is dipped in molten aluminum, iron and aluminum react to form a hard, brittle iron-aluminum layer at the interface. Silicon in the Type 1 bath slows that reaction and keeps the alloy layer thin, which improves adhesion and lets the sheet be formed into exhaust and appliance parts without the coating flaking. Type 2 has no silicon, so its alloy layer is thicker and the coating is heavier, but its outer layer of pure aluminum resists weathering better.

ASTM A463 coating designations

ASTM A463 names coatings by type and weight. As with galvanized and Galvalume, the number is the minimum total coating on both sides in hundredths of an ounce per square foot, by the triple spot test. T1-40 means Type 1 with at least 0.40 oz/ft² total; T2-65 means Type 2 with at least 0.65 oz/ft² total. Other weights exist, such as T1-25 and T2-100.

Aluminum is far lighter than zinc, so a given coating weight is much thicker. The approximate figures below are calculated from the triple spot minimum with an even split between sides, using densities of 2.66 g/cm³ for the Type 1 alloy and 2.70 g/cm³ for Type 2.

DesignationMin total, triple spotMin total, single spotApprox coating per side
T1-400.40 oz/ft² (about 122 g/m²)0.30 oz/ft²0.9 mil (23 µm)
T2-650.65 oz/ft² (about 198 g/m²)0.60 oz/ft²1.45 mil (37 µm)

Treat these thicknesses as estimates: the iron-aluminum layer next to the steel is denser than the outer coating, so producers publish somewhat lower figures, especially for Type 2. For context, G90 galvanized carries about 0.76 mil (19 µm) of zinc per side. A463 also defines the base steel, using familiar designations such as Commercial Steel (CS), Forming Steel (FS) and Structural Steel (SS), so a complete callout reads like ASTM A463 Type 1, CS Type B, T1-40, followed by thickness.

Heat resistance of aluminized steel

Heat is where Type 1 earns its place. The aluminum coating forms a thin, stable aluminum oxide film that resists scaling far better than bare steel. Type 1 aluminized steel is typically rated for oxidation resistance up to about 1250°F (677°C) in air. Above that range, the coating gradually converts into an iron-aluminum alloy that still slows scaling but loses its bright appearance.

Aluminized steel also reflects a large share of radiant heat while the surface stays bright, which helps in heat shields, oven liners and reflector panels. By comparison, zinc coatings are generally not recommended for continuous service above about 390°F (200°C), because the zinc begins to separate from the steel. That gap is why exhaust and combustion parts use aluminized or stainless steel rather than galvanized.

Choosing a material for hot parts

MaterialPractical temperature limit in air (typical)Relative cost
Galvanized steelAbout 390°F (200°C) continuousLowest
Type 1 aluminized steelAbout 1250°F (677°C)Low
304 stainless steelAbout 1600°F (870°C) intermittent, 1700°F (925°C) continuousHigh

These are oxidation and scaling limits, not strength ratings. Steel of any kind loses strength as it heats, so structural parts that run hot need a separate design check. Where the limit for aluminized steel is close, the usual next step is 304 stainless steel or another heat resisting stainless grade.

Tip: For parts that run hot and also see wet, salty or acidic condensate, compare aluminized steel with stainless before committing. Aluminized steel costs much less but is a coating; once it is consumed at hot spots, the base steel scales.

Corrosion behavior and cut edges

In ordinary air, aluminum forms a passive oxide that corrodes very slowly, which gives Type 2 its long life on roofs, walls and buried drainage structures. The trade-off is that aluminum is less sacrificial than zinc in neutral atmospheres. Cut edges, punched holes and deep scratches on aluminized sheet can show light rust staining because the coating does not protect bare steel as actively as galvanizing does.

In chloride environments such as marine air or road salt, aluminum becomes more active and does provide galvanic protection to exposed steel. Behavior varies with exposure, so in critical outdoor applications, plan for edge sealing or design cut edges to drain and dry.

Where aluminized steel is used

  • Type 1: automotive exhaust systems, mufflers and heat shields; oven cavities, range and grill components; water heater and furnace flues and combustion chambers; heat reflectors and ducts carrying hot air
  • Type 2: industrial roofing and siding; culverts and drainage structures; grain bins and agricultural buildings

Fabricating aluminized steel

Type 1 aluminized sheet bends, roll forms and draws well when bend radii are reasonable. In very tight bends, the hard alloy layer can crack and the outer coating may craze; this is normally cosmetic but can open small paths to the steel. Type 2, with its heavier coating, is better suited to moderate forming such as corrugating and panel profiles.

Aluminized steel can be laser cut, sheared and punched. It resistance welds well, and arc welding is possible, though aluminum entering the weld pool can affect bead quality, so removing the coating at the joint helps on structural welds. Welding aluminized sheet produces no zinc fume, but normal fume extraction is still required. After welding, the heated area loses its coating and is usually protected with a high temperature aluminum paint where appearance or corrosion matters.

Most aluminized parts are used bare. They can be painted after cleaning with a pretreatment suited to aluminum surfaces.

Store aluminized bundles dry and ventilated, as with any coated sheet. Moisture trapped between tight stacks can leave dark staining on the aluminum surface, which is mostly cosmetic but unwelcome on visible appliance and trim parts. When ordering, always state the type as well as the weight: a purchase order that says only “aluminized” leaves the mill or distributor to choose between two products with very different jobs.

For how aluminized compares with zinc and aluminum-zinc coatings, see what Galvalume is and what galvanized steel is.

Aluminized steel from ASA

Aluminized steel to ASTM A463 is on ASA’s coated steel stock list, alongside galvanized, galvannealed and Galvalume sheet in the flat-rolled sheet and plate line. Mill certifications and full material traceability are available. ASA can level and cut coated sheet to length, then laser cut, form and weld heat shields, housings and brackets in house.

Frequently asked questions

Is aluminized steel the same as aluminum?

No. Aluminized steel is carbon steel with a thin aluminum or aluminum-silicon coating on each side, so it has the strength, stiffness, weight and magnetism of steel. Solid aluminum sheet is a different metal, about one third the weight of steel, with lower stiffness and a different welding process. Aluminized steel costs less and handles heat far better than aluminum alloys.

How hot can aluminized steel get?

Type 1 aluminized steel is typically rated for oxidation resistance in air up to about 1250°F (677°C). Above that temperature, iron diffuses into the coating and turns it into an iron-aluminum alloy that still slows scaling but darkens and becomes brittle. For sustained higher temperatures or heavy thermal cycling, stainless steel is usually the better choice.

Will aluminized steel rust?

The aluminum coating itself does not rust, and it protects the steel well in normal air and in many hot environments. Rust can appear at cut edges, punched holes and deep scratches, where bare steel is exposed, because aluminum is less sacrificial than zinc in neutral conditions. Edge staining is usually light, but it is worth planning for on visible parts.

Can aluminized steel be painted?

Yes, although most aluminized parts are used bare because the coating already provides heat and corrosion resistance. To paint it, clean off oils, use a pretreatment or primer formulated for aluminum surfaces, and choose a coating rated for the service temperature. For hot parts, high temperature silicone paints are common; ordinary paints and powders will discolor or fail.

Why is aluminized steel used for exhaust systems?

Exhaust parts face high temperatures, thermal cycling and acidic condensate. Type 1 aluminized steel resists scaling at exhaust temperatures, tolerates condensate far better than bare steel, and forms easily into tubes, shells and heat shields. It does this at much lower cost than stainless steel, which is why it is widely used for mufflers, exhaust tubing and shields.

Material, processing and fabrication from one supplier

Send a drawing or a material list and the ASA team will quote it from stock.