On this page
A709 bridge steel is the ASTM specification for structural steel plates and shapes used in bridges. ASTM A709 (with AASHTO M 270 as its matching AASHTO specification) groups several grades in one standard, from Grade 36 through high performance steels with minimum yields up to 100 ksi (690 MPa), and adds fracture toughness requirements tied to the bridge member type and the coldest temperature the bridge will see.
Most A709 grades have the same strength as a familiar building specification: Grade 36 matches A36, Grade 50 matches A572 Grade 50, Grade 50S matches A992 and Grade 50W matches A588. What A709 adds is Charpy V-notch impact testing and tighter control for members whose failure could bring down a span.
A709 grades and strength
| A709 grade | Min yield | Tensile | Similar specification |
|---|---|---|---|
| 36 | 36 ksi (250 MPa) | 58 to 80 ksi (400 to 550 MPa) | A36 |
| 50 | 50 ksi (345 MPa) | 65 ksi (450 MPa) min | A572 Grade 50 |
| 50S (shapes) | 50 to 65 ksi (345 to 450 MPa) | 65 ksi (450 MPa) min | A992 |
| 50W | 50 ksi (345 MPa) | 70 ksi (485 MPa) min | A588 |
| HPS 50W | 50 ksi (345 MPa) | 70 ksi (485 MPa) min | None (high performance) |
| HPS 70W | 70 ksi (485 MPa) | 85 to 110 ksi (585 to 760 MPa) | None (high performance) |
| HPS 100W, to 2.5 in | 100 ksi (690 MPa) | 110 to 130 ksi (760 to 895 MPa) | None (high performance) |
The W suffix marks weathering grades, which can be used uncoated in suitable environments. The specification also includes quenched and self-tempered (QST) grades for heavy rolled shapes and a chromium-alloyed corrosion resistant plate grade, 50CR, for long-life applications. Values above are for the thickness ranges where each grade is most commonly used; some grades step down in strength for very thick plate, so check the current A709 table for heavy sections.
Toughness: the part that makes A709 a bridge steel
Bridges carry cyclic truck and rail loads for decades, often at low temperatures where steel becomes less tolerant of cracks. A709 addresses this with Charpy V-notch (CVN) impact requirements, which measure how much energy a notched sample absorbs at a specified test temperature.
The required energy and test temperature depend on two choices the bridge designer makes:
- Member type. Non-fracture-critical tension components carry a T designation. Fracture-critical members, whose failure could cause collapse (called nonredundant steel tension members in current AASHTO terminology), carry an F designation and have higher toughness requirements.
- Temperature zone. AASHTO divides the country by lowest anticipated service temperature. Zone 1 is 0°F (minus 18°C) and above; Zone 2 is below 0 to minus 30°F (minus 18 to minus 34°C); Zone 3 is below minus 30 to minus 60°F (minus 34 to minus 51°C).
A plate for a tension flange on a bridge in a Zone 2 state would be ordered as A709 Grade 50W with a T2 designation, for example. Material without a T or F designation, such as cross frames and other secondary members, is supplied to the base strength requirements without mandatory impact testing.
Tip: Copy the full designation from the contract plans to the purchase order, including grade, T or F, and zone. “A709 Grade 50” alone does not tell the mill which impact test to run, and the mill certification must show it.
High performance steel (HPS) grades
The HPS grades were developed in the 1990s through a cooperative program of the Federal Highway Administration, the US Navy and the American Iron and Steel Institute. The goal was steel with higher strength, much better toughness and easier weldability than conventional bridge grades. HPS 50W and HPS 70W are now widely used for plate girders, and HPS 70W in particular allows shallower or lighter girders and longer spans.
Weldability comes from very low carbon and sulfur. The table shows the chemistry limits for HPS 70W.
| Element | HPS 70W limit (wt%) |
|---|---|
| Carbon | 0.11 max |
| Manganese | 1.10 to 1.35 |
| Phosphorus | 0.020 max |
| Sulfur | 0.006 max |
| Silicon | 0.30 to 0.50 |
| Copper | 0.25 to 0.40 |
| Nickel | 0.25 to 0.40 |
| Chromium | 0.45 to 0.70 |
| Molybdenum | 0.02 to 0.08 |
| Vanadium | 0.04 to 0.08 |
Copper, nickel and chromium give HPS grades their weathering ability. The low carbon reduces the risk of hydrogen cracking, which allows lower preheat than conventional steels of the same strength. Conventional Grades 36, 50, 50S and 50W follow chemistry close to their building-specification counterparts.
Where A709 is used
- Plate girders, rolled beam girders and box girders for highway bridges
- Railroad bridge members, floor beams and stringers
- Cross frames, diaphragms, bearing stiffeners and connection plates
- Pedestrian bridges and long-span structures on public projects
- Non-bridge structures where the owner wants CVN-tested steel, such as heavy cold-service framing
State departments of transportation set their own preferences within A709, so the same element may be called 50W on one project and HPS 50W on another. Rolled beams for short spans are commonly Grade 50 or 50S; built-up plate girders increasingly use HPS 50W in the webs and HPS 70W in the flanges, a combination known as a hybrid girder.
Federally funded highway bridges also fall under the FHWA Buy America rule (23 CFR 635.410), which generally requires steel and iron permanently incorporated in the project to be melted and manufactured in the United States, with all coating and manufacturing processes performed domestically. Requirements and waivers vary by program, so confirm them with the contracting agency before ordering.
Fabricating A709 to the bridge code
Bridge steel is welded under AASHTO/AWS D1.5, the Bridge Welding Code, rather than AWS D1.1. D1.5 has stricter requirements for welding procedure qualification, consumable control, preheat and inspection, and fracture-critical work also requires a fracture control plan. Fabricators building main members commonly hold AISC certification for bridge work.
Cutting, drilling, punching limits, heat curving and cambering are all addressed by the governing bridge specifications. For mill material, the key fabrication issues are traceability, so every piece can be matched to the heat number and CVN results on its certification, and handling that avoids notches and gouges on tension members.
Weathering grades also follow the detailing advice in our guide to A588 weathering steel: drain water, avoid debris traps and specify weathering filler metals for exposed welds.
A709 compared with building grades
For building framing, there is usually no reason to pay for A709 when A992 steel or A36 steel will do. A709 earns its cost where impact toughness must be certified, where the owner’s specification requires it, or where an HPS grade’s strength saves weight. Because Grades 36, 50, 50S and 50W meet the strength requirements of their building counterparts, A709 material with a full mill certification can often be accepted in their place, subject to the engineer’s approval.
Buying A709 from ASA
American Steel & Aluminum stocks A709 in its structural shapes line along with A36, A992 and A588. Mill certifications and full material traceability are available, and ASA’s structural steel processing includes sawing, beam drilling and coping, plasma and oxy-fuel cutting of carbon plate up to 8 in thick, and welding. Call 1-800-933-7833 with the grade, designation and quantities on your plans.
Frequently asked questions
Is A709 the same as AASHTO M 270?
They are companion specifications covering the same bridge steels. ASTM publishes A709, and AASHTO publishes M 270 for use by state transportation departments, and the two are kept closely aligned. Contract documents may reference either one, sometimes both. When they differ in a particular revision, the specification named in the contract governs, so check which one the project cites.
What does 50W mean in A709 Grade 50W?
The 50 is the minimum yield strength in ksi, equal to 345 MPa. The W means the grade is a weathering steel, alloyed with copper, chromium and nickel so it can develop a protective patina and be left unpainted in suitable environments. Grade 50W has essentially the same strength and chemistry as ASTM A588.
What is the difference between T and F designations in A709?
Both add mandatory Charpy V-notch impact testing. T applies to tension components that are not fracture critical, and F applies to fracture-critical members, whose failure could cause collapse. F material has higher required impact energy and stricter testing frequency. The number after the letter, 1, 2 or 3, identifies the AASHTO temperature zone for the bridge site.
Can A709 steel be used for buildings?
Yes. A709 grades meet or exceed the strength requirements of the building specifications they parallel, so they are structurally suitable. They are rarely specified for buildings because the added toughness testing costs more and is not usually needed. Owners sometimes choose A709 for cold-service industrial structures or heavy framing where certified impact toughness is useful.