6061-T6 Aluminum: Properties and Uses

The most widely used heat-treatable aluminum alloy: 6061 chemistry, T6 and T651 properties, how it machines, bends and welds, and where it fits best.

Updated October 2026 5 min read By the ASA team

On this page
  1. 6061 aluminum composition
  2. What T6 and T651 mean
  3. 6061-T6 mechanical and physical properties
  4. Machining, bending and welding 6061
  5. Where 6061-T6 is used
  6. 6061 compared with other common aluminum alloys
  7. Buying 6061 aluminum from ASA

6061-T6 aluminum is a heat-treatable aluminum-magnesium-silicon alloy in its solution heat treated and artificially aged temper, and it is the most widely used general-purpose structural aluminum. Under ASTM B209, 6061-T6 sheet and 6061-T651 plate must reach at least 42 ksi (290 MPa) tensile strength and 35 ksi (240 MPa) yield strength in most thicknesses, with good corrosion resistance, very good machinability and good weldability.

That balance makes 6061 the default choice for frames, brackets, base plates, fixtures and machined parts, and it is available in more forms than almost any other alloy: sheet, plate, bar, rod, tube and extruded shapes. This guide covers the chemistry, what the temper letters mean, B209 and typical properties, how 6061 behaves in the shop and where another alloy is the better buy.

6061 aluminum composition

Chemistry limits for 6061 (UNS A96061) are registered by the Aluminum Association and required by ASTM B209 for sheet and plate, ASTM B221 for extrusions and ASTM B211 for cold finished bar.

ElementLimit (wt%)
Silicon0.40 to 0.8
Iron0.7 max
Copper0.15 to 0.40
Manganese0.15 max
Magnesium0.8 to 1.2
Chromium0.04 to 0.35
Zinc0.25 max
Titanium0.15 max
Other elements, each / total0.05 max / 0.15 max
AluminumRemainder

Magnesium and silicon combine during heat treatment to form magnesium silicide (Mg2Si), the fine precipitate that gives 6061 its strength. The small copper addition raises strength further, and chromium controls grain structure. Copper is kept low enough that corrosion resistance stays good, although not at the level of the 5xxx marine alloys.

What T6 and T651 mean

Unlike 3003 and 5052, which gain strength only from cold work, 6061 is strengthened by heat treatment. The temper designation tells you how the material was processed:

  • O (annealed): the softest condition, used when parts need severe forming before heat treatment.
  • T4: solution heat treated and naturally aged at room temperature. Noticeably softer than T6 and easier to bend.
  • T6: solution heat treated, quenched and then artificially aged at an elevated temperature. This is the full-strength condition for sheet and many extrusions.
  • T651: T6 plus stress relief by controlled stretching. Plate is normally supplied as T651 because the stretching removes quench stresses, so the plate stays flatter when it is machined.
  • T6511: the extrusion equivalent of T651, stretched and then lightly straightened.

For most buyers the practical choice is T6 for sheet, T651 for plate that will be machined, and T6 or T6511 for bar, tube and shapes. If a drawing simply says “6061-T6” for plate, T651 normally satisfies it, but confirm with the engineer when the drawing is controlled.

6061-T6 mechanical and physical properties

Specification minimums are what a mill certification must show. Typical values are averages useful for design comparison, not guarantees.

PropertyValueBasis
Tensile strength, sheet and plate (T6, T651)42 ksi (290 MPa) minASTM B209, most thicknesses up to 4 in
Yield strength, sheet and plate (T6, T651)35 ksi (240 MPa) minASTM B209
Tensile / yield, extrusions (T6, T6511)38 ksi (260 MPa) / 35 ksi (240 MPa) minASTM B221
Tensile strength45 ksi (310 MPa)Typical
Yield strength40 ksi (276 MPa)Typical
Elongation12 to 17%Typical, depends on specimen
Brinell hardness95 HBTypical
Shear strength30 ksi (207 MPa)Typical
Modulus of elasticity10,000 ksi (68.9 GPa)Typical
Density0.0975 lb/in³ (2.70 g/cm³)Typical

Minimum elongation in B209 varies with thickness, and plate thicker than 4 in carries a lower tensile minimum, so check the specification table for the exact size you are buying. To estimate part weights, use the aluminum sheet and plate weight chart. Remember that 6061 has about one third the stiffness of steel, so a part that must not deflect may need a deeper section rather than just a stronger alloy.

Machining, bending and welding 6061

Machining

6061-T6 is one of the most popular aluminum alloys for machining. It cuts cleanly, holds a good surface finish and does not smear the way softer alloys do, which is why T651 plate and T6 bar are standard stock for machined fittings, fixtures and manifolds. Its chips tend to be long and continuous, so sharp, positive-rake tooling and good chip control help. Annealed and T4 material machine less cleanly because they are gummy.

Bending and forming

In the T6 temper, 6061 is far less forgiving in a press brake than 5052. It needs a generous inside radius, typically around 1.5 to 3 times thickness for 1/8 in (3.2 mm) sheet and more for thicker material, and bends should run across the rolling direction where possible. Tight bends in T6 tend to crack on the outside of the radius. When a part needs tight bends, a common route is to form it in the O or T4 temper and then heat treat it to T6 after forming. The guide to bend allowance and K-factor covers how radius affects flat patterns.

Welding

6061 welds readily with GTAW (TIG) and GMAW (MIG), but it should always be welded with filler metal. Autogenous welds without filler are prone to hot cracking. ER4043 is the usual choice for crack resistance and good flow, and ER5356 gives higher shear strength and a better color match if the part will be anodized.

Welding heat removes the T6 strength next to the weld. AWS D1.2 uses a minimum as-welded tensile strength of 24 ksi (165 MPa) for 6061-T6 groove welds, well below the 42 ksi base metal minimum, so welded 6061 structures are designed around the weaker heat-affected zone. A full solution heat treatment and age after welding can restore most of the strength, but that is not practical for most assemblies. See welding stainless steel vs aluminum for more on aluminum welding practice.

Where 6061-T6 is used

  • Structural frames and brackets: machine frames, equipment bases, mounting brackets and supports, often built from extruded tube, angle and channel.
  • Machined parts: fixtures, tooling plates, manifolds, housings and fittings cut from T651 plate or T6 bar.
  • Transportation: truck and trailer components, ramps and walkways, where strength per pound matters.
  • Marine hardware: fittings, ladders and above-waterline structures, usually with anodizing or a coating for long service.
  • Industrial equipment: guards, rails, conveyor parts and enclosure framing.

Tip: If a part is mostly formed sheet with tight bends, and strength is not the main driver, 5052-H32 is usually easier and cheaper to fabricate. Reserve 6061 for parts that need strength, machining or extruded shapes.

6061 compared with other common aluminum alloys

AlloyStrengthened byWhere it fits
3003-H14Cold workLow cost, easy forming, lightly loaded sheet
5052-H32Cold workFormed sheet, enclosures, salt water exposure
6061-T6Heat treatmentStructural parts, machined parts, extrusions

For a side-by-side look at the two alloys most often compared, read 5052 vs 6061 aluminum. For how aluminum compares with steel on weight, strength and cost, see aluminum vs steel.

Buying 6061 aluminum from ASA

American Steel & Aluminum stocks 6061 aluminum, supplied with mill certifications and full material traceability. Give the form, temper, size and quantity on your request, and the quote will confirm availability. ASA can laser cut, saw, form, weld and powder coat 6061 parts under one company, with most JIT orders delivered in 24 to 48 hours from five Northeast locations. Request a quote or call 1-800-933-7833.

Frequently asked questions

What does T6 mean in 6061-T6?

T6 means the aluminum was solution heat treated, quenched and then artificially aged at an elevated temperature to reach full strength. The aging step forms fine magnesium silicide precipitates that more than double the strength of annealed 6061. Plate is usually sold as T651, which adds stretching to relieve quench stresses so it stays flat during machining.

Is 6061-T6 aluminum stronger than 5052?

Yes. ASTM B209 requires at least 42 ksi tensile and 35 ksi yield for 6061-T6 sheet, compared with 31 ksi tensile and 23 ksi yield for 5052-H32. The trade-off is formability and salt water resistance, where 5052 is better. Choose 6061 when strength and machining matter, and 5052 when parts are mostly bent sheet.

Can you bend 6061-T6 aluminum?

Yes, but it needs a larger inside bend radius than softer alloys, typically around 1.5 to 3 times thickness for 1/8 in sheet, and bends should run across the rolling direction. Tight bends in T6 often crack. For tight radii, form the part in the O or T4 temper and heat treat it to T6 afterward.

What filler metal is used to weld 6061 aluminum?

ER4043 and ER5356 are the two common fillers. ER4043 resists hot cracking and flows well, while ER5356 gives higher shear strength and a better color match after anodizing. Always use filler, because autogenous welds in 6061 are prone to cracking. Expect lower strength next to the weld, since welding heat removes the T6 temper locally.

Is 6061 aluminum good for marine use?

6061 has good corrosion resistance and is common for marine fittings, ladders and above-waterline structures, especially when anodized or coated. For hulls, tanks and parts in constant contact with salt water, 5xxx alloys such as 5052, 5083 and 5086 perform better because they contain almost no copper.

Material, processing and fabrication from one supplier

Send a drawing or a material list and the ASA team will quote it from stock.