On this page
5052 aluminum is an aluminum-magnesium alloy with about 2.5% magnesium, and in its H32 and H34 tempers it is considerably stronger than the other common general-purpose sheet alloys, 3003 and 5005. Under ASTM B209, 5052-H32 must reach a tensile strength of at least 31 ksi (215 MPa) and 5052-H34 at least 34 ksi (235 MPa), roughly 50 to 70% above the 3003-H14 minimum, while still forming and welding well.
Excellent resistance to salt water and marine atmospheres, good fatigue strength and easy fabrication make 5052 the default alloy for enclosures, fuel tanks, marine parts and formed structural sheet. This guide covers the chemistry, what separates H32 from H34, B209 and typical properties, fabrication notes and comparisons with neighboring alloys.
5052 aluminum composition
Chemistry limits for 5052 (UNS A95052) are registered by the Aluminum Association and required by ASTM B209 for sheet and plate.
| Element | Limit (wt%) |
|---|---|
| Silicon | 0.25 max |
| Iron | 0.40 max |
| Copper | 0.10 max |
| Manganese | 0.10 max |
| Magnesium | 2.2 to 2.8 |
| Chromium | 0.15 to 0.35 |
| Zinc | 0.10 max |
| Other elements, each / total | 0.05 max / 0.15 max |
| Aluminum | Remainder |
Magnesium is a strong solid solution strengthener in aluminum and does not reduce corrosion resistance, which is why the 5xxx series is the marine family. The small chromium addition controls grain structure and improves resistance to stress corrosion. Copper is held very low, an important reason 5052 performs so well in salt water.
Magnesium content also matters for service temperature. Alloys with more than about 3% magnesium, such as 5083 and 5086, can become sensitized to intergranular corrosion after long exposure above about 150°F (65°C). At 2.2 to 2.8% magnesium, 5052 stays below that threshold.
H32 vs H34: what the tempers mean
Both tempers are strain hardened by cold rolling and then given a low-temperature stabilizing treatment. Without it, strain-hardened aluminum-magnesium sheet slowly loses some strength over time at room temperature. The second digit sets the degree of hardening:
- H32 (quarter hard): the most common 5052 temper and the usual choice for parts that are press brake formed. It offers a good balance of strength and bendability.
- H34 (half hard): higher strength and stiffness against denting, with somewhat less formability. Common for flat or lightly formed panels, covers and parts where strength matters more than tight bends.
Annealed 5052-O is available for severe forming and deep drawing, and harder H36 and H38 tempers are used for some flat products.
Mechanical and physical properties
| Temper | B209 tensile | B209 min yield | Typical tensile | Typical yield |
|---|---|---|---|---|
| 5052-O | 25 to 31 ksi (170 to 215 MPa) | 9.5 ksi (65 MPa) | 28 ksi (193 MPa) | 13 ksi (90 MPa) |
| 5052-H32 | 31 to 38 ksi (215 to 265 MPa) | 23 ksi (160 MPa) | 33 ksi (228 MPa) | 28 ksi (193 MPa) |
| 5052-H34 | 34 to 41 ksi (235 to 285 MPa) | 26 ksi (180 MPa) | 38 ksi (262 MPa) | 31 ksi (214 MPa) |
B209 values are the specification requirements; the typical values are Aluminum Association figures for comparison. B209 minimum elongation varies with thickness. Typical elongation in 2 in for 1/16 in sheet is about 12% for H32 and 10% for H34. Typical fatigue endurance limits are 17 ksi (117 MPa) for H32 and 18 ksi (124 MPa) for H34, high for a non-heat-treatable alloy and one reason 5052 is used for parts that vibrate.
Physical properties (typical)
| Property | Typical value |
|---|---|
| Density | 0.097 lb/in³ (2.68 g/cm³) |
| Modulus of elasticity | 10,200 ksi (70.3 GPa) |
| Thermal conductivity at 77°F (25°C) | 138 W/m·K |
| Electrical conductivity | 35% IACS |
| Melting range | 1125 to 1200°F (607 to 649°C) |
With a density of 0.0968 lb/in³, 0.063 in 5052 sheet weighs about 0.88 lb/ft², 0.090 in about 1.25 lb/ft² and 0.125 in about 1.74 lb/ft² (thickness times 144 times density).
Fabricating 5052-H32 and H34
Press brake forming
5052-H32 is one of the most press-brake-friendly aluminum alloys in a strong temper, which is why sheet metal shops default to it for enclosures and brackets. Use an inside radius at least equal to the guidance for the thickness and temper; H34 needs larger radii than H32 and is more likely to crack on the outside of tight bends. Orient bend lines across the rolling direction where possible. Springback is higher than steel, so expect to over-bend slightly.
Welding
5052 welds well by TIG and MIG. 5356 is the most common filler, giving good strength and a reasonable color match; 4043 is also acceptable for some joints. The heat-affected zone anneals during welding and drops toward O temper strength, so welded H32 or H34 parts are not as strong near the weld as the base sheet. Clean the oxide layer immediately before welding to avoid porosity.
Cutting, machining and finishing
5052 laser cuts, punches and shears cleanly. It machines better than 3003 because it is harder, though less freely than heat-treated alloys. It anodizes with good protection but a slight yellowish tint, so for decorative clear anodize 5005 aluminum is better. 5052 takes paint and powder coating well after proper pretreatment.
Tip: 5052 cannot be heat treated to recover strength after welding or annealing. If a design needs full H32 strength at the joints, use mechanical fasteners, place welds in low-stress areas, or size the part around the as-welded strength.
Common uses of 5052 aluminum
- Electronic and electrical enclosures, chassis, cabinets and covers
- Battery and energy storage enclosures, doors and panels
- Fuel tanks for trucks, equipment and boats
- Marine parts: small boat hulls, hatches, consoles, decking and fittings
- Truck and trailer bodies, toolboxes and fenders
- Pressure vessels, hydraulic tubing and heat exchangers
- Appliance parts, signage blanks and formed brackets
In wet and marine service, the alloy is rarely the weak point; the joints are. Stainless steel or carbon steel fasteners in direct contact with 5052 set up a galvanic cell when salt water bridges them, and the aluminum corrodes around the fastener. Isolating washers and sealants, plus aluminum hardware where loads allow, prevent this. Crevices that hold salt water deserve the same attention.
For marine-grade material selection across steel and aluminum, see marine grade steel and aluminum for shipbuilding.
5052 compared with other aluminum alloys
| Alloy | Magnesium (wt%) | Where it fits |
|---|---|---|
| 3003-H14 | None (manganese alloy) | Lower cost, lower strength, easiest forming |
| 5005-H34 | 0.50 to 1.1 | Similar to 3003 in strength; best for decorative anodizing |
| 5052-H32 / H34 | 2.2 to 2.8 | Strong, formable, weldable; excellent in salt water |
| 5083 / 5086 | About 3.5 to 4.9 | Higher strength marine plate and welded hulls |
Choose 5052 over 3003-H14 aluminum when the part carries load, flexes, or sees salt water. When a part needs more strength or heavy machining, compare 5052 vs 6061 aluminum. Choose a 5083 or 5086 marine plate for large welded hull structures, and consider 5052 for most formed sheet parts below that.
Buying 5052 from ASA
American Steel & Aluminum stocks 5052-H32 and 5052-H34 in its flat rolled sheet and plate line, with stock list specifications including ASTM B209, ASME SB-209, AMS 4015, 4016 and 4017, and AMS-QQ-A-250/8. Mill certifications and full material traceability are available, and ASA can laser cut, press brake form, weld and powder coat 5052 parts. Most JIT orders are delivered in 24 to 48 hours from five Northeast locations.
Frequently asked questions
Is 5052 aluminum marine grade?
Yes, 5052 is widely considered a marine-grade alloy because its magnesium alloying and very low copper give excellent resistance to salt water and salt spray. It is common for small boat hulls, fuel tanks, hatches and fittings. Larger welded hulls and structures usually move up to higher-strength marine alloys such as 5083 or 5086 in plate thicknesses.
Which bends better, 5052-H32 or 5052-H34?
5052-H32 bends better. As the quarter-hard temper it has lower yield strength and more elongation than half-hard H34, so it tolerates tighter inside radii without cracking. H34 is chosen when extra strength and dent resistance matter more than forming. For very tight bends or deep draws, the annealed O temper is the safest option.
Can 5052 aluminum be heat treated?
Not to increase strength. 5052 is a non-heat-treatable alloy that gains strength only from magnesium in solution and cold work. Heating it to annealing temperatures softens it toward the O temper. The stabilizing step in H32 and H34 tempers is a low-temperature treatment that locks in properties, not a strengthening heat treatment.
What do AMS 4016 and AMS 4017 cover?
They are SAE Aerospace Material Specifications for 5052 aluminum sheet and plate in specific tempers: AMS 4016 covers H32 and AMS 4017 covers H34, while AMS 4015 covers the annealed O temper. Aerospace and defense drawings often call these out instead of, or alongside, ASTM B209, adding their own testing and certification requirements.
Is 5052 stronger than 3003?
Yes, by a clear margin. The B209 minimum tensile strength is 31 ksi for 5052-H32 compared with 20 ksi for 3003-H14, and 5052 has much higher fatigue strength. It also performs better in salt water. 3003 costs less and forms slightly more easily, so it remains a good choice for lightly loaded ductwork, liners and trim.