On this page
5005 aluminum is a low-magnesium, non-heat-treatable aluminum alloy best known for anodizing well. It has strength similar to 3003, good formability and weldability, and better corrosion resistance in many atmospheres, but its real advantage is a clean, uniform anodized finish, which is why it is the standard sheet alloy for architectural panels, trim and visible anodized parts.
The alloy is most often supplied in H32 or H34 tempers, and an anodizing quality version is produced specifically for decorative finishing. This guide covers 5005 chemistry, tempers and typical properties, why it anodizes better than 3003, fabrication tips and how it compares with its neighbors.
5005 aluminum composition
5005 (UNS A95005) is an Aluminum Association registered alloy; the limits below are the registered values that ASTM B209 sheet and plate must meet.
| Element | Limit (wt%) |
|---|---|
| Silicon | 0.30 max |
| Iron | 0.7 max |
| Copper | 0.20 max |
| Manganese | 0.20 max |
| Magnesium | 0.50 to 1.1 |
| Chromium | 0.10 max |
| Zinc | 0.25 max |
| Other elements, each / total | 0.05 max / 0.15 max |
| Aluminum | Remainder |
5005 is the leanest common member of the 5xxx (aluminum-magnesium) series. Its magnesium content of roughly 0.8% gives about the same strength that 3003 gets from 1.0 to 1.5% manganese. The difference is what those elements do in the anodic film: magnesium stays in solution and anodizes clear, while the manganese-bearing particles in 3003 cloud the film.
Tempers and mechanical properties
Like other 5xxx alloys, 5005 is strengthened only by cold work. Its common tempers are:
- O: annealed, for maximum formability.
- H32 and H34: strain hardened and stabilized, quarter hard and half hard. Stabilizing is a low-temperature thermal treatment that prevents the slow age softening magnesium alloys can show at room temperature.
- H12 and H14: strain hardened only, quarter and half hard; slightly higher yield than the matching H3x temper, with less elongation.
| Temper (typical) | Tensile strength | Yield strength | Elongation in 2 in |
|---|---|---|---|
| 5005-O | 18 ksi (124 MPa) | 6 ksi (41 MPa) | 25% |
| 5005-H32 | 20 ksi (138 MPa) | 17 ksi (117 MPa) | 11% |
| 5005-H34 | 23 ksi (159 MPa) | 20 ksi (138 MPa) | 8% |
| 5005-H14 | 23 ksi (159 MPa) | 22 ksi (152 MPa) | 6% |
These are Aluminum Association typical values for 1/16 in thick sheet, intended for comparison. ASTM B209 sets the guaranteed minimum yield and tensile range for each temper and thickness, and those are the values that appear on the mill certification. Note that H34 and H14 reach similar tensile strength, but H34 keeps more elongation, which is one reason the H3x tempers are preferred for formed architectural parts.
Physical properties (typical)
| Property | Typical value |
|---|---|
| Density | 0.098 lb/in³ (2.70 g/cm³) |
| Modulus of elasticity | 10,000 ksi (69 GPa) |
| Electrical conductivity | 52% IACS |
| Melting range | 1170 to 1210°F (632 to 654°C) |
Using a density of 0.0975 lb/in³, 0.063 in 5005 sheet weighs about 0.88 lb/ft² and 0.125 in sheet about 1.76 lb/ft² (thickness times 144 times density).
Why 5005 is the anodizing alloy
Anodizing grows a thick, hard aluminum oxide layer from the surface of the part. The layer is translucent, so anything in the metal shows through it. In 5005, the alloying magnesium stays dissolved and the film comes out clear and even, giving a bright, consistent finish for clear anodize and a true color for dyed or electrolytically colored finishes.
That consistency matters on buildings and products where many parts sit side by side. Architectural sheet in 5005 is widely used because its anodized appearance matches 6063 architectural extrusions, so panels, trim, mullions and framing can be finished together and look like one material. Mills produce anodizing quality (often abbreviated AQ) 5005 with tighter control of surface condition and chemistry for exactly this purpose.
Architectural anodizing in North America is usually specified to AAMA 611, which defines two film thickness classes. Class I calls for an anodic coating of at least 0.7 mil (18 µm) and is the usual choice for exterior storefronts and curtain walls with heavy exposure. Class II covers 0.4 to 0.7 mil (10 to 18 µm) and is common for interior and lower-exposure exterior work. The alloy, temper, film class and color should all be on the drawing so the sheet, the extrusions and the anodizer are working to the same requirement.
Tip: For matched anodized work, order all panels for one elevation from the same lot and anodize them together. Even anodizing quality sheet can vary slightly in tone from lot to lot, and differences in grain direction show after finishing, so keep panels oriented the same way.
Fabricating 5005
Forming
5005 forms about as easily as 3003. H32 and H34 bend cleanly on a press brake and roll-form well for panel profiles. Bend radius guidance from the Aluminum Association increases with temper and thickness, and O and H32 tolerate tighter bends than H34.
Welding
5005 welds readily by TIG and MIG. For parts that will be anodized after welding, 5356 filler gives a closer color match; 4043 filler turns dark gray when anodized and stands out. As with any strain-hardened alloy, the weld zone softens toward O temper strength.
Cutting and surface care
Laser cutting, shearing and punching are routine. Because the finished surface is the product, protect 5005 with PVC film through cutting and forming, avoid scratches and steel contamination, and remove any flux or residue before anodizing. Handling marks that are invisible on bare metal often become visible after anodizing.
Common uses of 5005 aluminum
- Architectural wall panels, spandrels, column covers and curtain wall infill
- Anodized trim, fascia, soffits and storefront components
- Signage, letters and display fixtures
- Appliance and electronics faceplates, control panels and bezels
- Lighting fixtures and decorative housings
- Electrical conductor applications that make use of its good conductivity
5005 is also painted and coil coated, but if a part will be painted rather than anodized, 3003 often costs less and performs similarly. See architectural steel and aluminum for how alloy and finish choices work together on building projects.
5005 vs 3003 and 5052
| Factor | 3003-H14 | 5005-H34 | 5052-H32 |
|---|---|---|---|
| Main alloying element | Manganese | Magnesium (low) | Magnesium (2.2 to 2.8%) |
| Typical tensile strength | 22 ksi (150 MPa) | 23 ksi (159 MPa) | 33 ksi (228 MPa) |
| Decorative anodizing | Fair, slight gray or yellow cast | Excellent | Good, slightly yellowish |
| Salt water resistance | Good | Good | Excellent |
| Best for | Ductwork, tanks, general sheet | Anodized architectural and visible parts | Higher strength, marine, enclosures |
For deeper detail on the neighbors, read 3003-H14 aluminum and 5052-H32 and H34 aluminum.
Buying 5005 from ASA
American Steel & Aluminum stocks 5005 aluminum in its flat rolled sheet and plate line, with ASTM B209 and ASME SB-209 among its stock list specifications and mill certifications available. Its leveling and cut-to-length line processes aluminum from 0.032 to 0.125 in with PVC film or interleaving to protect finish-critical surfaces, and ASA can laser cut and form panels before delivery. Call 1-800-933-7833 to discuss temper, thickness and finish requirements.
Frequently asked questions
Why is 5005 aluminum used for anodizing?
Its magnesium alloying stays dissolved in the aluminum and anodizes into a clear, uniform oxide film, so finished parts look bright and consistent. Alloys with more manganese, iron or silicon particles, such as 3003, produce a cloudier or tinted film. 5005 anodized sheet also matches the color of 6063 architectural extrusions, which designers rely on for coordinated building finishes.
What is the difference between 5005-H32 and 5005-H34?
Both are strain hardened and then stabilized. H32 is quarter hard and H34 is half hard, so H34 has higher yield and tensile strength and slightly lower elongation. H32 suits parts with tighter bends or more forming; H34 suits flat panels that need more stiffness against dents and oil-canning. Both anodize equally well.
Is 5005 aluminum stronger than 3003?
They are close. In half-hard tempers, typical tensile strength is about 23 ksi for 5005-H34 and 22 ksi for 3003-H14, so the strength difference is small enough that the choice is usually made on finish and cost rather than strength. Designs that need meaningfully more strength in a formable sheet usually move up to 5052.
Can 5005 aluminum be used outdoors without a finish?
Yes. 5005 resists atmospheric corrosion well and is used bare in many exterior applications. Unfinished, it gradually dulls and can develop light pitting in coastal or industrial air. For architectural work, it is usually anodized or painted, which keeps its appearance consistent for decades and makes cleaning easier. Avoid contact with wet concrete, mortar and steel.