  1. 430 stainless steel composition
  2. Mechanical and physical properties
  3. 2B and BA finishes on 430
  4. Corrosion resistance and where 430 fits
  5. Fabricating 430 stainless
  6. 430 compared with other stainless grades
  7. Buying 430 stainless from ASA

430 stainless steel is a ferritic stainless grade with about 16 to 18% chromium and almost no nickel (0.75% max). It is magnetic, costs less than 304, and offers good resistance to mild corrosion and oxidation, which makes it the standard choice for appliance panels, trim and indoor decorative sheet.

Most 430 sheet is sold in one of two cold rolled finishes: 2B, a smooth, moderately reflective mill finish, and BA (bright annealed), a highly reflective, near mirror surface. This guide covers the ASTM A240 chemistry and properties, what separates the two finishes, where 430 works and where it does not, and how to fabricate it.

430 stainless steel composition

430 is designated UNS S43000 and is roughly equivalent to EN 1.4016. ASTM A240 sets the chemistry for flat-rolled 430 sheet, strip and plate.

ElementASTM A240 limit (wt%)
Carbon0.12 max
Manganese1.00 max
Silicon1.00 max
Phosphorus0.040 max
Sulfur0.030 max
Chromium16.0 to 18.0
Nickel0.75 max
IronBalance

The absence of meaningful nickel is the whole story of 430. Without nickel, the steel keeps a ferritic (body-centered cubic) structure at all temperatures, the same basic structure as carbon steel. That is why it is magnetic, why it cannot be hardened by heat treatment, and why its price moves less with the nickel market than austenitic grades do.

Chromium still forms the passive oxide film that defines stainless steel, so 430 resists staining in clean indoor air and many mild environments. With less chromium than 304, almost no nickel and no molybdenum, its protection is thinner and easier to break down.

Mechanical and physical properties

Mechanical properties (annealed)

PropertyASTM A240 requirement
Tensile strength65 ksi (450 MPa) min
Yield strength (0.2% offset)30 ksi (205 MPa) min
Elongation in 2 in (50 mm)22% min
Hardness89 HRB (183 HBW) max

The yield minimum matches 304, but tensile strength and elongation are lower. The 22% elongation figure is the one to watch in fabrication: 430 bends and stretches well, but it does not have the reserve ductility that lets 304 survive deep draws. It also work hardens far less than 304, so formed areas stay closer to their original strength.

Physical properties (typical)

PropertyTypical value
Density0.280 lb/in³ (7.75 g/cm³)
Modulus of elasticity29,000 ksi (200 GPa)
Mean thermal expansion, 32 to 212°F (0 to 100°C)5.8 µin/in·°F (10.4 µm/m·°C)
Thermal conductivity at 212°F (100°C)15.1 Btu/hr·ft·°F (26.1 W/m·K)
Magnetic responseStrongly magnetic

430 expands about 40% less than 304 when heated and conducts heat better. In practice that means less warping during welding and laser cutting, and better behavior in parts that cycle between hot and cold, such as range hoods and heater trim.

2B and BA finishes on 430

ASTM A480 defines the standard finishes for stainless sheet. For 430, two of them cover most orders.

FinishHow it is madeAppearanceTypical use
2BCold rolled, annealed, pickled, then given a light pass on polished rollsSmooth, uniform, moderately reflective grayHidden or painted parts, liners, brackets, parts that will be polished later
BA (bright annealed)Cold rolled on highly polished rolls, then annealed in a controlled atmosphere so no scale formsBright, highly reflective, close to a mirrorAppliance fronts, decorative trim, reflectors, visible panels

The difference comes from the annealing step. A 2B coil is annealed in air and then pickled in acid to remove scale, which leaves a slightly matte surface that the final roll pass smooths but does not brighten. A BA coil is annealed in a protective gas atmosphere, so the surface never oxidizes and keeps the polish from the rolls.

BA is the finish to specify when the part is the product’s face and you do not want to pay for polishing. 2B costs less, hides minor handling marks better and is a good base for brushed or No. 4 polishing, painting and powder coating.

Tip: Order BA sheet with a protective PVC film or paper interleaving and leave the film on through cutting and forming. A reflective surface shows every scratch, and repairing BA is far harder than protecting it.

Corrosion resistance and where 430 fits

430 handles indoor air, clean water, many foods, detergents and mild organic acids well. It also resists nitric acid and has useful oxidation resistance at elevated temperatures. As a ferritic grade it is far less prone to chloride stress corrosion cracking than 304, which matters in some hot water and heat exchanger designs.

Its limit is chloride pitting. Outdoors, especially near salt water or road salt, 430 develops rust spots and tea staining much sooner than 304 or 316. It is best treated as an indoor and sheltered-exterior grade.

  • Good fit: kitchen appliances, dishwasher and washer interiors, range hoods, indoor architectural trim, decorative panels, automotive interior trim.
  • Use with care: sheltered exterior parts that are washed regularly.
  • Poor fit: coastal sites, splash zones, pool environments, chlorinated or salty process water.

Because it is magnetic, 430 also works where 304 cannot: induction cookware bases, magnetic latches and assemblies that use magnets for holding or sensing. For a side by side look at cost, corrosion and magnetism, see 304 vs 430 stainless steel.

Fabricating 430 stainless

Cutting and forming

430 cuts cleanly on fiber lasers and shears, and its lower thermal expansion keeps flat blanks flat. It forms well in bending and shallow stretch forming, with less springback than 304. Deep draws are harder: the lower elongation limits draw depth, and 430 can show roping (fine surface ridges parallel to the rolling direction) on heavily stretched areas, which matters on BA parts.

Ferritic steels lose toughness at low temperatures, so heavier gauges of 430 are best formed at room temperature or slightly warm rather than cold in an unheated shop in winter.

Welding

430 is weldable but needs more care than austenitic grades. Heat causes grain growth near the weld, which reduces ductility and toughness in the heat-affected zone. Thin sheet is usually TIG or resistance welded with low heat input. Austenitic fillers such as ER308L or ER309L give a more ductile weld; a matching 430 filler gives a better color match. Heavier sections are often preheated to roughly 300 to 450°F (150 to 230°C) and annealed after welding at around 1450°F (790°C) to restore ductility (typical practice). Many 430 appliance parts avoid fusion welding entirely and use spot welds, rivets, clinching or fasteners.

Heat treatment and machining

430 cannot be hardened by quenching. It is supplied annealed and is only strengthened by cold work. It machines more like carbon steel than 304 does, with less gumming and work hardening, so tool life is better.

430 compared with other stainless grades

GradeStructureKey difference from 430
430Ferritic, magneticBaseline: 16 to 18% Cr, 0.75% Ni max
304Austenitic, nonmagnetic annealedAdds 8 to 10.5% nickel; better corrosion resistance, ductility and weldability
316Austenitic, nonmagnetic annealedAdds nickel and 2 to 3% molybdenum; for chlorides and marine exposure

Choose 430 when the environment is indoor or sheltered, the part is formed rather than deep drawn, and appearance or magnetism matters more than maximum corrosion resistance. Step up to 304 stainless steel for welded assemblies, deep draws and general outdoor use. Our guide on how to choose a stainless steel grade walks through the decision.

Buying 430 stainless from ASA

American Steel & Aluminum stocks 430 stainless in both 2B and BA finishes as part of its stainless sheet and plate line, with mill certifications and full material traceability. Its Alcos 6-high leveling and cut-to-length line handles stainless from 24 to 10 gauge and can apply PVC film or interleaving to protect finished surfaces. ASA can then laser cut, form and deliver parts from five Northeast locations; call 1-800-933-7833 to discuss your order.

Frequently asked questions

Is 430 stainless steel magnetic?

Yes. 430 is a ferritic stainless steel, so it is strongly magnetic in every condition, annealed or cold worked. A magnet will grip it about as firmly as carbon steel. This is a quick way to tell it apart from annealed 304 or 316, although a magnet test alone is not proof of grade; the mill certification is.

Will 430 stainless steel rust outdoors?

It can. 430 has less chromium than 304, almost no nickel and no molybdenum, so rain, humidity and especially salt break down its protective film sooner. Inland, sheltered exterior trim that is washed regularly can perform acceptably. Near the coast or where deicing salt is used, expect rust spots and staining, and specify 304 or 316 instead.

What is the difference between 430 2B and 430 BA?

Both are cold rolled and annealed. 2B is annealed in air, pickled to remove scale and lightly rolled, giving a smooth gray surface with moderate shine. BA is annealed in a protective atmosphere so it never scales, keeping a bright, highly reflective surface. BA suits visible decorative panels; 2B suits hidden, painted or later-polished parts.

Can 430 stainless steel be hardened by heat treatment?

No. 430 stays ferritic at all temperatures, so quenching does not form the hard martensite that hardenable grades such as 410 or 440C produce. The only way to raise its strength is cold work, such as rolling or forming. Heat treatment of 430 is limited to annealing, which softens the metal and restores ductility after welding or heavy forming.

Is 430 stainless safe for food contact?

430 is widely used for food-contact surfaces such as appliance interiors, cookware bodies and utensils, because it resists most foods, detergents and mild acids. For salty, acidic or chloride-rich foods, brines, and harsh sanitizing chemicals, 304 or 316 hold up better. Confirm the requirements of the applicable food equipment standard for your product.

Material, processing and fabrication from one supplier

Send a drawing or a material list and the ASA team will quote it from stock.