On this page
In 316 vs 316L stainless steel, the only chemical difference is carbon: 316 allows up to 0.08%, while 316L is limited to 0.030%. Both carry the same 2 to 3% molybdenum and resist chlorides equally in the annealed condition. The low carbon of 316L keeps weld zones from sensitizing, so it is the standard choice for welded parts in marine, chemical and pharmaceutical service.
The trade-off is a 5 ksi lower guaranteed strength for 316L, which dual-certified 316/316L removes. Because most 316 is bought precisely for aggressive environments, the L decision tends to matter more here than it does between 304 and 304L.
316 vs 316L side by side
| Property | 316 | 316L |
|---|---|---|
| UNS number | S31600 | S31603 |
| Approx EN equivalent | 1.4401 | 1.4404 |
| Carbon, max | 0.08% | 0.030% |
| Chromium | 16.0 to 18.0% | 16.0 to 18.0% |
| Nickel | 10.0 to 14.0% | 10.0 to 14.0% |
| Molybdenum | 2.00 to 3.00% | 2.00 to 3.00% |
| Nitrogen, max | 0.10% | 0.10% |
| Tensile strength, min | 75 ksi (515 MPa) | 70 ksi (485 MPa) |
| Yield strength (0.2% offset), min | 30 ksi (205 MPa) | 25 ksi (170 MPa) |
| Elongation in 2 in, min | 40% | 40% |
| Hardness, max | 95 HRB (217 HBW) | 95 HRB (217 HBW) |
| PREN, typical | About 23 to 25 | About 23 to 25 |
| Weld zone, as welded | Can sensitize | Resists sensitization |
Chemistry and mechanical values are ASTM A240 limits for annealed sheet, strip and plate; PREN is a typical value. Manganese, silicon, phosphorus and sulfur limits are the same for both. Physical properties such as density, 0.289 lb/in³ (8.00 g/cm³), and thermal expansion are the same as well.
Why the L matters more for 316
Sensitization is the formation of chromium carbides at grain boundaries when stainless steel is held at roughly 800 to 1500°F (425 to 815°C), as the metal beside a weld is. The carbides rob the surrounding metal of chromium and leave narrow paths that corrode first.
Whether a sensitized zone actually fails depends on the environment. In dry indoor air it may never matter. In seawater, brine, chloride sanitizers, or sulfuric and phosphoric acids, it is where attack begins. Those are exactly the services 316 is bought for. Paying for molybdenum and then losing corrosion resistance at every weld defeats the purpose, which is why welded 316 equipment is specified as 316L almost by default.
Some industries formalize this. Bioprocessing and pharmaceutical owners commonly require 316L for product contact surfaces, often with additional limits on sulfur so automated orbital welds penetrate consistently from heat to heat. Chemical plant specifications typically call for 316L on any welded vessel or skid, and naval and marine programs follow the same logic for welded hardware exposed to salt.
316 also starts from a slightly higher carbon ceiling than 304 (0.08% versus 0.07%), so a standard 316 heavy section has a little more carbon available to form carbides. For full background on how low carbon prevents this, see 316L stainless steel.
Where standard 316 still fits
- Parts that are not welded: sheared, laser cut, formed or machined parts, fasteners and fittings. Without a weld thermal cycle there is nothing to sensitize.
- Thin sheet with short single-pass welds: thin material cools through the sensitizing range in seconds, so standard 316 usually performs well.
- Parts annealed after fabrication: solution annealing dissolves any carbides formed during welding.
- Elevated temperature strength: carbon helps austenitic stainless hold strength when hot. For load-bearing parts in sustained high temperature service, 316 or 316H is generally preferred over 316L.
- Code designs that use 316 allowables: pressure equipment designed to the higher 316 allowable stresses needs material that meets 316 strength, which dual-certified 316/316L also provides.
Dual certification and alternatives
Most flat-rolled 316L produced today is dual certified as 316/316L: carbon at or below 0.030% with nitrogen and other elements balanced to meet 316’s 75 ksi tensile and 30 ksi yield minimums. The mill test report shows both grades. For buyers, that means one material covers drawings calling for either grade, and the price difference between them on dual-certified sheet and plate is usually small.
Specify “316/316L dual certified” when a welded part is designed to 316 strength, and check the carbon, tensile and yield results on the mill test report when material arrives. Otherwise a callout for 316L alone may legitimately be filled with material that meets only the lower 316L minimums.
Some European drawings call for 316Ti (EN 1.4571), which controls sensitization a different way: titanium ties up carbon as titanium carbide so chromium carbides cannot form. It serves the same purpose as 316L in welded parts. In North American supply, 316L is far more widely stocked, so confirm with the designer whether 316L is an acceptable substitute before ordering 316Ti.
Tip: A marine or process weldment can be built to 316L and still corrode at the welds if heat tint is left on. Put weld cleaning and passivation on the drawing alongside the grade.
When to choose 316 or 316L
| Part or service | Specify |
|---|---|
| Unwelded coastal panels, covers and trim | 316 or 316/316L |
| Marine weldments, railings and deck hardware assemblies | 316L |
| Chemical tanks, vessels and process skids | 316L |
| Pharmaceutical and biotech equipment | 316L |
| Food equipment with brines or chloride sanitizers, welded | 316L |
| Welded parts designed to 316 strength | 316/316L dual certified |
| Load-bearing parts at sustained high temperature | 316 or 316H |
When the part is welded and wet, 316L is the safer specification. When the environment is mild, the better question is whether you need 316 at all; see 304 vs 316 stainless steel.
Beyond the L: what else decides weld corrosion
Low carbon solves one problem. Three others cause most of the weld corrosion seen on 316L equipment:
- Heat tint: the colored oxide beside a weld is less protective than the natural passive film. Remove it by pickling, mechanical cleaning or electropolishing, then passivate to ASTM A967 or the practices in ASTM A380.
- Iron contamination: carbon steel brushes, grinding dust and shared fixtures embed iron that rusts and starts pits. Keep tooling dedicated to stainless.
- Crevices: lap joints, intermittent welds and gasketed seams trap chloride solutions. Continuous, full-penetration welds and drainable designs last longer than any grade upgrade, and they are easier to clean and inspect over the life of the equipment.
Use ER316L filler for both grades so the weld deposit carries matching molybdenum. Welds normally contain a little ferrite to prevent hot cracking, which is why a magnet may cling slightly to a 316L weld bead even though the plate is nonmagnetic.
Buying 316 and 316L from ASA
ASA stocks 316 and 316L stainless in its sheet and plate line, with mill certifications, full material traceability and DFARS documentation available. For marine and naval programs, ASA supplies marine-grade materials to defense and shipbuilding customers and can laser cut, form and weld 316L parts in house. Note any dual-certification requirement on your quote request so the certification can be checked against it.
Frequently asked questions
Is 316L weaker than 316?
Its guaranteed minimums are lower: 70 ksi tensile and 25 ksi yield for 316L, compared with 75 ksi and 30 ksi for 316 under ASTM A240. Actual mill results are often close for both. Most 316L sold as sheet and plate is dual certified, meaning it also meets the 316 minimums, so in practice many parts see no strength penalty at all.
Can 316L be used where a drawing calls for 316?
Usually, if the material is dual certified 316/316L, because it then meets both the chemistry and the strength of 316. Straight 316L is acceptable where the design does not depend on 316 minimum strength, but the substitution should be approved by whoever owns the drawing. The reverse, using 316 where 316L is specified, is generally not acceptable for welded parts.
Should marine weldments be made from 316 or 316L?
316L. Boat and dock hardware, railings, brackets and shipboard assemblies are typically welded and then exposed to salt spray or splash, which is exactly where a sensitized weld zone corrodes first. 316L avoids that without post-weld annealing. Pair it with ER316L filler, remove heat tint, and passivate for the best result in salt exposure.
What is 316Ti?
316Ti is a titanium-stabilized version of 316, designated EN 1.4571 in Europe. Titanium combines with carbon before chromium can, so welds resist sensitization even though carbon is not held as low as in 316L. It serves a similar purpose to 316L and is common in European specifications, while 316L is far more widely stocked in North America.
Is there a price difference between 316 and 316L?
Typically very little. Because mills produce most flat-rolled material as dual certified 316/316L, distributors stock one product for both grades. Prices for either move with nickel and molybdenum surcharges, which change monthly, so compare current quotes for the same thickness, finish and quantity rather than expecting a fixed premium.