3003-H14 Aluminum: Properties and Uses

The general-purpose aluminum sheet: 3003-H14 chemistry, ASTM B209 strength, what the half-hard temper means, how it forms and welds, and when to choose 5005 or 5052.

Updated October 2026 5 min read By the ASA team

On this page
  1. 3003 aluminum composition
  2. What H14 means
  3. Mechanical and physical properties
  4. Fabricating 3003-H14
  5. Common uses of 3003-H14 aluminum
  6. 3003-H14 vs other aluminum sheet alloys
  7. Buying 3003-H14 from ASA

3003-H14 aluminum is a manganese-alloyed aluminum in the half-hard, strain-hardened temper, and it is one of the most widely used general-purpose aluminum sheet products. It is typically about 20% stronger than commercially pure 1100 aluminum, forms and welds easily, and resists corrosion well, which makes it a standard choice for ductwork, tanks, panels, trim and enclosures.

Under ASTM B209, 3003-H14 sheet and plate must have a tensile strength of 20 to 26 ksi (140 to 180 MPa) and a minimum yield strength of 17 ksi (115 MPa). This guide explains the chemistry, what H14 means, typical properties, fabrication behavior and when to choose 3003 over 5005 or 5052.

3003 aluminum composition

The Aluminum Association registers the chemistry of 3003 (UNS A93003), and ASTM B209 applies those limits to sheet and plate.

ElementLimit (wt%)
Silicon0.6 max
Iron0.7 max
Copper0.05 to 0.20
Manganese1.0 to 1.5
Zinc0.10 max
Other elements, each / total0.05 max / 0.15 max
AluminumRemainder

Manganese is the main alloying element of the 3xxx series. It strengthens the aluminum moderately without hurting corrosion resistance or formability much. Because 3003 gets no strength from heat treatment, it is classed as a non-heat-treatable alloy: the only ways to raise its strength are alloying and cold work.

What H14 means

Aluminum temper designations describe how the metal was processed after casting and rolling. For non-heat-treatable alloys like 3003:

  • O is fully annealed, the softest and most formable condition.
  • H1x means strain hardened only, by cold rolling after the final anneal.
  • The second digit gives the degree of hardening: 2 is quarter hard, 4 half hard, 6 three-quarter hard and 8 full hard.
  • H2x tempers are strain hardened past the target and then partially annealed back down. H24 has similar strength to H14 with somewhat better elongation.

H14 is the most common commercial temper because it balances stiffness and dent resistance against formability. It is firm enough to hold flat as a panel and soft enough to bend, roll and lightly draw.

Mechanical and physical properties

Mechanical properties

PropertyASTM B209 requirementTypical value
Tensile strength20 to 26 ksi (140 to 180 MPa)22 ksi (150 MPa)
Yield strength17 ksi (115 MPa) min21 ksi (145 MPa)
ElongationMinimum varies with thickness8% in 2 in (1/16 in sheet)
Shear strengthNot specified14 ksi (97 MPa)
Brinell hardnessNot specified40 HB

Typical values are Aluminum Association figures for guidance; the mill certification reports actual results. B209 sets a maximum tensile strength as well as a minimum for H14, so material that is too hard to form fails the specification just as material that is too soft does.

Physical properties (typical)

PropertyTypical value
Density0.099 lb/in³ (2.73 g/cm³)
Modulus of elasticity10,000 ksi (69 GPa)
Thermal conductivity (H14) at 77°F (25°C)159 W/m·K
Electrical conductivity (H14)41% IACS
Melting range1190 to 1210°F (643 to 654°C)

At about one third the density of steel, 3003-H14 sheet is light to handle. Weight per square foot equals thickness in inches times 144 times the density in lb/in³. Using 0.0986 lb/in³, 0.063 in sheet weighs about 0.89 lb/ft² and 0.125 in sheet about 1.78 lb/ft². The modulus is also one third of steel’s, so an aluminum panel of the same thickness deflects about three times as much under the same load. For more sizes, see the aluminum sheet and plate weight chart.

Fabricating 3003-H14

Forming

3003-H14 bends well on a press brake and rolls easily into cylinders, gutters and duct. Thin gauges can typically be bent with an inside radius close to the material thickness or less, and heavier gauges need larger radii. Springback is greater than with mild steel because of the lower modulus. For deep draws or severe stretch forming, the O temper is the better starting point.

Welding

3003 is one of the easiest aluminum alloys to weld by TIG or MIG, with 4043 or 1100 filler commonly used, and 5356 also an option. The heat of welding anneals the material next to the weld, so the heat-affected zone drops close to O temper strength. Designs that rely on H14 strength should account for that local softening.

Cutting and machining

The alloy shears, punches and laser cuts cleanly. Fiber lasers handle aluminum’s reflectivity well, and nitrogen assist gas gives a bright, oxide-free edge. 3003 is soft and gummy to machine compared with harder alloys; sharp tools with high rake angles and lubrication help.

Finishing

3003 can be anodized for protection, painted, powder coated and brushed. Its manganese content gives anodized surfaces a slightly gray or yellowish cast, so for decorative clear or color anodizing where appearance must match across parts, 5005 aluminum is the usual choice.

Tip: Keep aluminum separate from steel during storage and fabrication. Steel dust or chips embedded in the surface cause pitting and rust staining, and contact between bare aluminum and steel in wet service invites galvanic corrosion.

Common uses of 3003-H14 aluminum

  • HVAC ductwork, plenums, heat exchanger fins and coil housings
  • Fuel and storage tanks, chemical and food handling equipment
  • Truck and trailer panels, toolboxes and liners
  • Roofing, siding, gutters and flashing
  • Electronic chassis, enclosures, covers and brackets
  • Signs, trim, cooking utensils and appliance parts

Corrosion resistance explains much of this list. 3003 forms a stable oxide film that protects it in ordinary atmospheres, fresh water, many foods and a range of mild chemicals, and the manganese addition does little to weaken that protection. It does not need paint to survive indoors or in most inland outdoor settings, which keeps the cost of ductwork, tanks and liners down. Strongly alkaline or acidic cleaners and constant salt exposure are the conditions to avoid with bare 3003.

3003 is also a common base alloy for aluminum tread plate, which is covered in the guide to tread plate and diamond plate.

3003-H14 vs other aluminum sheet alloys

Alloy and temperTypical tensile strengthBest for
3003-H1422 ksi (150 MPa)General fabrication, ductwork, tanks, low cost formable sheet
5005-H3423 ksi (160 MPa)Architectural panels and parts that will be anodized
5052-H3233 ksi (230 MPa)Higher strength, marine and fuel tank service, enclosures

Typical values are Aluminum Association figures. Choose 3003-H14 when cost, formability and weldability matter more than strength. Step up to 5052 when the part carries load, sees salt water, or needs better fatigue resistance.

Buying 3003-H14 from ASA

American Steel & Aluminum stocks 3003-H14 sheet in its flat rolled sheet and plate line, to ASTM B209 and ASME SB-209. Its Alcos 6-high leveling line cuts aluminum from 0.032 to 0.125 in thick to length with PVC film or interleaving, and ASA can laser cut, form and weld the blanks into parts. Most JIT orders are delivered in 24 to 48 hours.

Frequently asked questions

Is 3003-H14 aluminum good for bending?

Yes. 3003-H14 is one of the more formable aluminum sheet products in a firm temper, and it bends well on a press brake in common sheet thicknesses. Heavier gauges need larger inside radii than thin ones. If a part needs very tight bends, deep draws or severe stretching, ordering the annealed O temper avoids cracking, at the cost of lower strength.

Can 3003 aluminum be heat treated?

Not to increase strength. 3003 is a non-heat-treatable alloy, so it does not respond to solution heat treating and aging the way 2xxx, 6xxx or 7xxx alloys do. Its strength comes from manganese and cold work. Heating it does anneal it, softening H14 toward the O temper, which is useful when a part needs re-forming.

Is 3003-H14 aluminum suitable for outdoor use?

Yes. 3003 develops a protective oxide film and resists weathering well, which is why it is used for roofing, siding, gutters and trailer panels. Coastal and industrial environments can cause pitting and dulling over time, and painted, anodized or coil-coated finishes extend appearance life. For direct salt water exposure, 5052 performs better.

What filler metal is used to weld 3003 aluminum?

4043 and 1100 are the most common filler metals for welding 3003 to itself. 4043 flows well and resists hot cracking, while 1100 gives a softer, more ductile weld. 5356 can also be used when higher weld strength is wanted. The heat-affected zone softens toward annealed strength regardless of filler choice.

Material, processing and fabrication from one supplier