On this page
1074 and 1075 steel are high carbon steels with 0.70 to 0.80% carbon, used mainly as spring steel in the form of cold rolled strip. After hardening and tempering they combine high strength and a large elastic range with enough toughness to flex repeatedly without breaking, which suits flat springs, clips, retaining rings, blades and saw plate.
The two grades have the same carbon range and differ only slightly in manganese, so they are often treated as interchangeable. Their properties depend almost entirely on condition: soft and formable when annealed, hard and springy when hardened and tempered. This guide covers the chemistry, typical properties, heat treatment, fabrication and how they compare with other carbon steels.
Chemical composition
SAE J403 sets the chemistry for both grades. 1074 is UNS G10740 and 1075 is UNS G10750.
| Element (wt%) | 1074 | 1075 |
|---|---|---|
| Carbon | 0.70 to 0.80 | 0.70 to 0.80 |
| Manganese | 0.50 to 0.80 | 0.40 to 0.70 |
| Phosphorus | 0.030 max | 0.030 max |
| Sulfur | 0.050 max | 0.050 max |
| Iron | Balance | Balance |
The slightly higher manganese in 1074 gives it marginally better hardenability, which can help in thicker strip. For most thin spring parts, the difference does not change the design, and mills and distributors often stock one or both under a combined 1074/1075 description. ASTM A684 is the common specification for cold rolled high carbon strip in these grades.
Properties by condition
High carbon strip is sold in two very different conditions, and choosing the right one is the most important ordering decision. The values below are typical; actual hardness is agreed with the mill and reported on the certification.
| Condition | Typical hardness | Approximate tensile strength | Used for |
|---|---|---|---|
| Annealed (spheroidized) | Soft; in the Rockwell B range | Low enough to blank and form | Parts that are stamped and formed, then heat treated |
| Hardened and tempered | About 40 to 50 HRC | About 180 to 250 ksi (1240 to 1720 MPa) | Flat springs and blades made from pre-tempered strip |
| As quenched (before tempering) | Roughly 60 HRC or higher in thin sections | Not used in service | Intermediate step only; too brittle |
Tensile values for hardened strip are approximate conversions from hardness, not measured minimums. Spheroidize annealing turns the carbides in the steel into small rounded particles, which is what makes such a high carbon grade soft enough for tight forming and progressive die work.
Pre-tempered strip (often sold as spring tempered, and sometimes with a blue or bright finish) is the faster route for simple flat springs, since the part needs only cutting and light forming. Annealed strip is the better route for complex formed shapes that would crack if bent hardened.
Physical properties (typical)
| Property | Typical value |
|---|---|
| Density | 0.284 lb/in³ (7.85 g/cm³) |
| Modulus of elasticity | 29,000 ksi (200 GPa) |
The modulus of elasticity barely changes with heat treatment, so a hardened spring is no stiffer than an annealed blank of the same size. What hardening adds is yield strength, which lets the spring deflect much further before it takes a permanent set.
Heat treating 1074 and 1075
Parts formed from annealed strip are hardened and tempered after fabrication. Typical practice is:
- Austenitize at roughly 1475 to 1525°F (800 to 830°C), in a protective atmosphere where possible to prevent decarburization.
- Quench in oil. Water is too severe for most thin, high carbon parts and causes cracking and distortion.
- Temper promptly, typically in the 600 to 900°F (315 to 480°C) range for spring hardness, adjusted to hit the target Rockwell C value.
Austempering, in which parts are quenched into a molten salt bath and held until they transform to bainite, is also widely used for 1074 and 1075 clips and springs. It produces good toughness at spring hardness with less distortion than oil quenching and tempering. Whatever the method, a decarburized surface lowers fatigue life, so surface carbon control matters on springs.
Tip: Specify hardness as a range, such as a 4-point HRC window, rather than a single number. It gives the heat treater a workable target and gives inspection a clear pass or fail.
Fabrication notes
Cutting
Annealed strip shears, blanks and laser cuts readily. Hardened strip can be laser cut, but the cut edge reheats and requenches, leaving a thin heat-affected zone with different hardness than the body of the part. On fatigue-critical springs, that edge can start cracks, so many spring makers blank in the annealed state and heat treat afterward, or finish edges by grinding or tumbling.
Forming
Bend annealed strip across the rolling direction where possible, with an inside radius generous enough for the thickness. Hardened strip needs much larger radii and springs back far more; tight bends in hardened material crack. Edge condition matters too: burrs and slit-edge roughness concentrate stress, so deburred or rounded edges are common on springs.
Welding and machining
These grades are generally not welded. The heat-affected zone forms brittle martensite on cooling, and welding destroys the temper of hardened parts. Where joining is unavoidable, mechanical fastening, riveting or carefully controlled spot welding on annealed material are typical. Machining is practical in the annealed condition; hardened material is ground.
Common uses
- Flat springs, leaf springs for light equipment and spring fingers
- Clips, retaining rings, spring washers and fastener clips
- Circular saw plate, scraper and doctor blades, trowels and putty knives
- Knives and cutting tools that need a durable edge with toughness
- Agricultural and lawn equipment blades and tines
- Latches, detents and lock springs in hardware and appliances
Plain carbon spring steel rusts, so finished parts are usually oiled, black oxided, painted or plated. Electroplating hardened springs introduces a risk of hydrogen embrittlement, which can cause sudden cracking under load days after plating; plated high-strength parts are normally baked soon after plating to drive the hydrogen out. Where a spring must survive wet or corrosive service without a coating, a stainless spring temper is the usual alternative to 1074 and 1075.
How 1074 and 1075 compare
| Grade | Carbon (wt%) | Character |
|---|---|---|
| 1050 | 0.48 to 0.55 | Tougher, easier to form, lower hardness; moderate springs and blades |
| 1074 / 1075 | 0.70 to 0.80 | Balanced spring steel: high strength with good toughness |
| 1095 | 0.90 to 1.03 | Highest hardness and wear resistance, less tough; fine edges and high stress springs |
Alloy spring steels such as 5160 and 6150 add chromium, or chromium and vanadium, for deeper hardening in thick sections and better fatigue performance in heavy springs. For lighter-duty parts, see 1050 steel; for the medium carbon option that welds more easily, see 1045 steel.
Buying 1074 and 1075 from ASA
American Steel & Aluminum lists C1074 and C1075 among the carbon steels in its flat rolled sheet and plate line, and ASTM A684 appears on its stock list specifications. Mill certifications and full material traceability are available, and ASA can laser cut, shear and deburr blanks before delivery from five Northeast locations. Request a quote with thickness, width, condition and hardness range.
Frequently asked questions
Is 1075 steel good for springs?
Yes. 1075 is one of the most common carbon spring steels for flat springs, clips and washers. Hardened and tempered to roughly the 40s to around 50 HRC, it has a high elastic limit and enough toughness to survive repeated flexing. For heavy, thick springs, alloy grades such as 5160 harden more deeply and resist fatigue better.
What is the difference between 1074 and 1075 steel?
Only manganese. Both contain 0.70 to 0.80% carbon, but 1074 has 0.50 to 0.80% manganese while 1075 has 0.40 to 0.70%. The extra manganese gives 1074 slightly higher hardenability. For most thin strip springs and blades the grades perform the same, and they are frequently stocked and supplied under a combined designation.
Can you bend 1075 spring steel?
In the annealed condition, yes, with a reasonable inside radius and the bend line across the rolling direction. That is how most formed springs and clips are made before heat treatment. Hardened and tempered strip is much less forgiving: it accepts only gentle bends, springs back strongly and cracks if bent sharply, especially parallel to the grain.
Is 1075 steel good for knives?
It is a popular choice for machetes, outdoor knives and swords because it is tough and sharpens easily. At 0.70 to 0.80% carbon it reaches lower peak hardness than 1095, so it holds a fine edge for less time but resists chipping and breaking better. Its plain carbon chemistry means blades need oiling or a coating to prevent rust.