On this page
1050 steel is a plain carbon steel with about 0.50% carbon, at the upper end of the medium carbon range. Compared with 1045 it offers a little more strength, hardness and wear resistance after heat treatment, at the cost of somewhat lower ductility and weldability, which makes it a common choice for blades, wear parts, flat springs and hardened machine components.
1050 has no single specification minimum for strength. Its properties are set by its condition: hot rolled, cold rolled or cold drawn, annealed, or hardened and tempered. Below are the SAE chemistry, typical values by condition, how it is heat treated and fabricated, and how to decide between 1050 and its neighbors.
1050 steel composition
1050 is designated UNS G10500, with SAE J403 setting its chemistry.
| Element | SAE J403 limit (wt%) |
|---|---|
| Carbon | 0.48 to 0.55 |
| Manganese | 0.60 to 0.90 |
| Phosphorus | 0.030 max |
| Sulfur | 0.050 max |
| Iron | Balance |
The carbon window overlaps 1045 (0.43 to 0.50%) at its low end, and the manganese range is the same. On nominal values, 1050 carries about 0.05% more carbon than 1045. That small increase raises the hardness achievable on quenching and the strength of the as-rolled material, and it moves the grade measurably closer to spring and blade applications.
Typical mechanical properties
These are typical values for bar product. They are not specification minimums, and they change with section size and processing. Rely on the mill certification for actual results and put required hardness or strength on the drawing.
| Condition (typical) | Tensile strength | Yield strength | Elongation | Hardness |
|---|---|---|---|---|
| Hot rolled | 90 ksi (620 MPa) | 49.5 ksi (340 MPa) | 15% | 179 HB |
| Cold drawn | 100 ksi (690 MPa) | 84 ksi (580 MPa) | 10% | 197 HB |
Each strength and hardness figure is roughly 10% above typical data for 1045 in the same condition, while elongation is slightly lower. Annealed 1050 is softer than either row in the table and is the condition to order for heavy forming or machining before hardening. Hardened and tempered 1050 covers a wide band of hardness depending on the tempering temperature: as quenched, thin sections can approach about 60 HRC, and tempering brings that down to the range a blade, wear part or spring needs.
Flat-rolled 1050 is also supplied as annealed cold rolled strip for parts that are blanked and formed first, then heat treated, and in some cases as pre-hardened and tempered strip. Hardness ranges for strip are agreed with the mill rather than fixed by the grade.
Heat treatment
1050 is hardened by heating into the austenite range, typically around 1475 to 1550°F (800 to 845°C), and quenching. Water or brine gives the highest as-quenched hardness and is used for heavier sections; oil is gentler and reduces cracking and distortion on thin parts and strip, at the cost of some hardness. Temper immediately after quenching.
- Low temper, roughly 300 to 450°F (150 to 230°C) typical: keeps high hardness for cutting edges and wear surfaces.
- Medium temper, roughly 600 to 900°F (315 to 480°C) typical: a spring and impact range, trading hardness for toughness.
- High temper, roughly 1000 to 1200°F (540 to 650°C) typical: tough machine parts with moderate hardness.
Like 1045, 1050 has low hardenability, so only thin sections and surfaces harden fully. Flame and induction hardening are widely used on 1050 shafts, rolls, sprockets and wear faces. For large sections that need uniform hardness throughout, an alloy grade is the better route.
Tip: Decarburization (loss of surface carbon) in hot rolled stock or during heat treatment leaves a soft skin that ruins edge hardness. Allow stock for grinding, or heat treat in a protective atmosphere, on any 1050 part where surface hardness is critical.
Fabricating 1050
Cutting and forming
Annealed 1050 strip and sheet can be blanked, laser cut and bent, but it needs larger inside bend radii than mild steel and more forming force. Grain direction matters: orient critical bends across the rolling direction where possible. Thermally cut edges harden as they cool, so plan secondary drilling or forming near cut edges carefully, or anneal first.
Machining
1050 machines adequately in the annealed or normalized state, a little harder on tools than 1045. Hardened 1050 is usually finished by grinding.
Welding
Welding 1050 is possible but demanding. Higher carbon means a harder, more crack-prone heat-affected zone than 1045, so preheat, low-hydrogen consumables, slow cooling and stress relief are all typically required, with preheat increasing with section size. In many designs, mechanical fastening or welding to a lower carbon component away from highly stressed areas is the practical answer. Hardened 1050 should not be welded without a qualified procedure.
Specifying 1050 on an order
Because the grade alone does not fix properties, a complete 1050 order states more than the number:
- Product form: hot rolled, hot rolled pickled and oiled, or cold rolled
- Condition: as rolled, annealed (often spheroidize annealed for forming), or hardened and tempered with a hardness range
- Thickness, width and length, plus any flatness or edge requirements
- Mill certification and traceability requirements
Leaving the condition off is the most common cause of parts that crack in the press brake or will not harden as expected.
Where 1050 steel is used
- Agricultural tillage tools, mower and cutter blades, and scraper edges
- Flat springs, clips and spring washers in moderate duty service
- Wear strips, chain and conveyor wear parts, guides and liners
- Shafts, axles, rolls and sprockets that are flame or induction hardened
- Hand tools and implements that need a hardened working edge
- Knives and industrial cutting tools where extreme hardness is not needed
1050 earns its place in parts that wear or flex, where 1045 is slightly short on hardness and a high carbon grade would be more brittle or harder to form than the part needs.
1050 vs 1045 and high carbon grades
| Factor | 1045 | 1050 | 1074 / 1075 |
|---|---|---|---|
| Carbon (wt%) | 0.43 to 0.50 | 0.48 to 0.55 | 0.70 to 0.80 |
| Hardened hardness | Good | Slightly higher | Highest of the three |
| Ductility and toughness | Best of the three | Moderate | Lowest when hardened |
| Weldability | Fair, with preheat | Limited | Generally not welded |
| Typical role | Shafts, pins, induction hardened parts | Blades, wear parts, moderate springs | Springs and edge parts |
If weldability or toughness is the concern, step down to 1045 steel. If you need spring performance or a longer-lasting edge, compare 1074 and 1075 high carbon steel. For general fabricated structures, a low carbon grade or HSLA steel gives strength without the heat treatment and welding complications.
Buying 1050 from ASA
American Steel & Aluminum lists C1050 among the hot rolled and cold rolled carbon steels in its flat rolled sheet and plate line, with mill certifications and full material traceability. ASA can laser cut and shear blanks, and its other processing services include machining, heat treating and deburring. Call 1-800-933-7833 to discuss thickness, condition and quantity.
Frequently asked questions
Is 1050 steel good for knives and blades?
It works well for tough, easily sharpened blades such as machetes, mower blades, tillage tools and large choppers, where impact resistance matters more than holding a very fine edge. At about 0.50% carbon it cannot reach the hardness of 1075, 1095 or tool steels, so for fine cutting edges and long edge life a higher carbon grade is usually chosen.
Can 1050 steel be used for springs?
Yes, for moderate-duty flat springs, clips and spring washers. Hardened and tempered to a medium hardness, 1050 has useful elastic range and good toughness. For springs that are highly stressed or must survive many cycles, higher carbon spring steels such as 1074, 1075 or 1095 are usually specified because they reach higher strength after tempering.
What is the difference between 1045 and 1050 steel?
1050 carries about 0.05% more carbon, with carbon ranges of 0.48 to 0.55% versus 0.43 to 0.50% for 1045. That gives 1050 slightly higher as-rolled strength and hardened hardness, plus better wear resistance. 1045 is a little more ductile, tougher and easier to weld and machine, which is why it dominates for shafts while 1050 is common for blades.
Does 1050 steel rust?
Yes. 1050 is a plain carbon steel with no chromium, so it rusts readily when exposed to moisture. Parts are usually oiled, painted, powder coated, black oxided or plated for protection. Blades and tools are often kept lightly oiled. Where corrosion resistance is required alongside hardness, a hardenable stainless steel is the alternative.