On this page
1045 steel is a medium carbon steel with about 0.45% carbon, giving it noticeably higher strength and hardness than mild steel while staying reasonably machinable. It can be hardened by heat treatment, most often by induction or flame hardening of the surface, which is why it is a standard material for shafts, pins, gears and wear parts.
Unlike structural grades, 1045 has no single specified minimum strength. Its properties depend on how it was produced and treated: hot rolled, cold drawn, annealed, normalized or hardened and tempered. This guide gives the SAE chemistry, typical properties by condition, heat treatment and welding notes, and where 1045 fits against lower and higher carbon grades.
1045 steel composition
1045 is designated UNS G10450. SAE J403 sets its chemistry.
| Element | SAE J403 limit (wt%) |
|---|---|
| Carbon | 0.43 to 0.50 |
| Manganese | 0.60 to 0.90 |
| Phosphorus | 0.030 max |
| Sulfur | 0.050 max |
| Iron | Balance |
The carbon range is what defines the grade. At 0.43 to 0.50% carbon, 1045 has enough carbon to form hard martensite when quenched, but its plain carbon chemistry gives it low hardenability: only a shallow layer, or a small section, will harden fully. That limitation is also an advantage, because it makes 1045 ideal for selective surface hardening over a tough core.
Mechanical properties by condition
The values below are typical, not specification minimums, and they vary with section size. Actual results are reported on the mill certification, and parts that need a guaranteed strength or hardness should state it on the drawing.
| Condition (typical) | Tensile strength | Yield strength | Elongation | Hardness |
|---|---|---|---|---|
| Hot rolled | 82 ksi (565 MPa) | 45 ksi (310 MPa) | 16% | 163 HB |
| Cold drawn | 91 ksi (625 MPa) | 77 ksi (530 MPa) | 12% | 179 HB |
- Annealed: the softest and most ductile condition, used when 1045 must be heavily machined or formed before hardening. Strength and hardness fall below the hot rolled values.
- Normalized: a more uniform, refined grain structure with strength somewhat above hot rolled, often used as a starting point before induction hardening.
- Hardened and tempered: strength and hardness depend on the tempering temperature and the section size. Induction or flame hardened surfaces typically reach the mid to upper 50s HRC.
Cold drawing raises yield strength the most, by about 70% over hot rolled in typical data, while reducing elongation. That makes cold drawn 1045 a good choice for parts that need strength and accuracy without heat treatment.
Physical properties (typical)
| Property | Typical value |
|---|---|
| Density | 0.284 lb/in³ (7.85 g/cm³) |
| Modulus of elasticity | 29,000 ksi (200 GPa) |
| Magnetic response | Ferromagnetic |
Heat treating 1045
1045 responds to all the common carbon steel heat treatments. The temperatures below are typical starting points; follow the heat treater’s procedure for the part and section size.
| Process | Typical temperature | Purpose |
|---|---|---|
| Annealing | 1450 to 1550°F (790 to 845°C), slow furnace cool | Soften for machining and forming |
| Normalizing | About 1600 to 1650°F (870 to 900°C), air cool | Refine grain, even out properties |
| Hardening | 1475 to 1550°F (800 to 845°C), water or brine quench; oil for thin parts | Form martensite for strength and wear resistance |
| Tempering | 400 to 1200°F (205 to 650°C) | Trade hardness for toughness after hardening |
Because water quenching a plain carbon steel is severe, sharp corners, holes and sudden section changes can crack. Generous radii and uniform sections help. For larger parts that need hardness all the way through, an alloy steel such as 4140 is usually a better choice than 1045.
Induction hardening is where 1045 is most at home. A coil heats only the surface of a shaft journal, gear tooth or wear face, and a water spray quenches it. The result is a hard, wear resistant case a fraction of an inch deep over a core that keeps the toughness of the normalized or hot rolled condition.
Machining, forming and welding
Machining
1045 machines well in the hot rolled, normalized or annealed condition, though more slowly than free machining grades such as 1117 or 12L14. Cold drawn 1045 gives a better surface finish and holds size well. Machine before hardening where possible, and finish grind hardened surfaces.
Forming and cutting
1045 is less ductile than mild steel, so it needs larger bend radii and more press force, and it is more likely to crack on the outside of a tight bend. Bend lines running perpendicular to the rolling direction tolerate tighter radii than bend lines parallel to it. Thermal cutting by laser, plasma or oxy-fuel leaves a hardened edge; anneal or machine that edge if the part will be drilled, tapped or formed near it.
Welding
1045 is weldable with precautions. Its carbon content means the heat-affected zone can harden and crack on cooling, especially in thick sections or under restraint. Typical practice is a preheat of roughly 300 to 500°F (150 to 260°C), increasing with thickness, low-hydrogen filler metal, controlled interpass temperature, slow cooling and often a post-weld stress relief. Welding hardened 1045 is not recommended without a qualified procedure.
Tip: If a part needs to be both welded and hardened, sequence it carefully: weld in the annealed or normalized condition, stress relieve, then harden only the areas that need it, ideally away from the welds.
Common uses of 1045 steel
- Shafts, axles, spindles and couplings
- Gears, sprockets, cams and pinions, often induction hardened
- Pins, bolts, studs and keys
- Hydraulic cylinder rods, usually induction hardened and chrome plated
- Wear strips, guides, clutch plates and machine components cut from flat stock
- Agricultural and construction equipment parts that see moderate wear and impact
In each of these, 1045 is chosen because it gives significantly more strength and wear resistance than mild steel at a modest cost, with the option of surface hardening exactly where wear happens.
In flat-rolled form, 1045 sheet and strip are used for parts that are blanked or laser cut to shape and then hardened: wear plates, scraper and cutter blades, washers, clutch and brake components, and brackets that must resist wear or deformation. Ordering annealed or hot rolled material keeps cutting and forming manageable, and heat treatment after fabrication sets the final hardness.
1045 compared with neighboring grades
| Grade | Carbon (wt%) | When to choose it |
|---|---|---|
| 1010 / 1018 | 0.08 to 0.20 | Formed and welded parts, carburized parts; easiest to weld |
| 1045 | 0.43 to 0.50 | Shafts and parts that need strength or induction hardening |
| 1050 | 0.48 to 0.55 | Slightly higher hardness and wear resistance; blades and wear parts |
| 1074 / 1075 | 0.70 to 0.80 | Springs and edge-holding parts, hardened and tempered |
For the lower carbon side, see 1006, 1008 and 1010 low carbon steel. Moving up in carbon, 1050 steel and 1074 and 1075 high carbon steel trade weldability and ductility for higher hardness.
Buying 1045 from ASA
C1045 is on American Steel & Aluminum’s carbon steel stock list in hot rolled and cold rolled product, and ASA also carries carbon steel bar in flats, squares and rounds. Mill certifications and full material traceability are available. ASA’s processing includes sawing, laser and plasma cutting, machining and heat treating; call 1-800-933-7833 to discuss the size, condition and quantity you need.
Frequently asked questions
What is 1045 steel used for?
1045 is used where a part needs more strength and wear resistance than mild steel at a reasonable cost. Typical examples are shafts, axles, gears, sprockets, pins, studs, hydraulic rods and machine components. Many of these are induction hardened only on their wear surfaces, so the working face is hard while the rest of the part stays tough.
How hard can 1045 steel get?
After induction or flame hardening, 1045 surfaces typically reach the mid to upper 50s on the Rockwell C scale. Through-hardening is limited to small sections because the plain carbon chemistry has low hardenability. Tempering reduces hardness in exchange for toughness, so the final value depends on the tempering temperature chosen for the application.
Is 1045 the same as C45 or S45C?
They are close equivalents rather than identical grades. C45 (EN 1.0503) in European standards and S45C in Japanese standards have similar carbon and manganese ranges to 1045, and they are often substituted for one another. Small differences in residual element limits and specified properties exist, so confirm suitability before replacing one with another on critical parts.
Is 1045 steel stronger than A36?
Yes, in typical condition. Hot rolled 1045 typically shows yield strength around 45 ksi and tensile strength around 82 ksi, compared with A36 minimums of 36 ksi yield and 58 ksi tensile. 1045 can also be hardened, which A36 cannot. The trade-off is weldability: A36 welds easily, while 1045 needs preheat and careful procedures.