Steel Plate for Shipbuilding: Grades and Processing

The hull plate grades shipyards specify, what the letters and numbers mean, how much plate weighs, and how it is cut, beveled, formed and prepared for welding.

Updated October 2026 5 min read By the ASA team

On this page
  1. Hull structural steel grades
  2. Naval plate and other specifications
  3. Plate weights for planning
  4. Cutting and edge preparation
  5. Forming, straightening and surface preparation
  6. Plate processing from ASA

Most steel plate for shipbuilding is hull structural steel to ASTM A131 or classification society rules, in ordinary strength grades such as A, B, D and E or higher strength grades such as AH36, DH36 and EH36. The number gives the minimum yield strength level and the letter gives the Charpy impact test temperature, so a plate’s grade tells you both how strong it is and how cold it can get before toughness becomes a concern.

Once it reaches the yard or fabricator, ship plate is cut with CNC plasma or oxy-fuel, beveled for welding, formed, blasted and primed, with the heat number carried onto every part. This guide covers both the grades and the processing.

Hull structural steel grades

ASTM A131, Standard Specification for Structural Steel for Ships, and the rules of classification societies such as ABS use the same grade designations. Strength levels are grouped as follows:

Strength groupMinimum yield strengthTensile strength range
Ordinary strength (A, B, D, E)34 ksi (235 MPa)58 to 75 ksi (400 to 520 MPa)
Higher strength 32 (AH32, DH32, EH32, FH32)46 ksi (315 MPa)64 to 85 ksi (440 to 590 MPa)
Higher strength 36 (AH36, DH36, EH36, FH36)51 ksi (355 MPa)71 to 90 ksi (490 to 620 MPa)
Higher strength 40 (AH40, DH40, EH40, FH40)57 ksi (390 MPa)74 to 94 ksi (510 to 650 MPa)

The letter sets the Charpy V-notch test temperature:

LetterImpact test temperature
A (ordinary strength)Generally not required in common thicknesses
B32 F (0 C), where testing applies
AH (higher strength)32 F (0 C)
D and DHminus 4 F (minus 20 C)
E and EHminus 40 F (minus 40 C)
FHminus 76 F (minus 60 C)

Required impact energy, testing frequency, thickness limits and heat treatment condition vary with grade and thickness, so use the specification and class rules for exact values. Grade A covers much of the lightly stressed structure on many vessels, while AH36 and DH36 are common for main hull girder strength members. Toughness grades D and E are typically assigned to critical locations such as sheer strakes, bilge strakes and structure in cold service. The naval architect assigns grades by location in the hull.

Navy combatants use specialized plate beyond the commercial grades. HY-80 and HY-100, covered by MIL-S-16216, are quenched and tempered alloy steels named for their nominal minimum yield strengths in ksi. They are very tough but demand careful preheat and heat input control during welding. HSLA-80 and HSLA-100, covered by MIL-S-24645, were developed to reach similar strength with easier welding and reduced preheat. Naval auxiliaries and many government vessels also use ASTM A131 grades such as DH36.

All of these alloyed naval steels can fall under the DFARS specialty metals rules because of their nickel, chromium or molybdenum content, so origin documentation matters as much as chemistry. Confirm the clauses that apply to your order with the buyer or contracting officer. Our guide to mil-spec metals covers how these specifications fit with AMS and ASTM documents.

Plate for classed vessels usually has to be produced at an approved mill and tested under the society’s survey, with the certificate stamped or endorsed accordingly. ASTM A131 plate also carries general requirements from ASTM A6, which sets thickness, flatness and marking tolerances for structural plate.

Plate weights for planning

Plate weight drives crane capacity, handling and freight. The table uses a steel density of 0.2836 lb/in³ (7.85 g/cm³):

Weight (lb/ft²) = thickness (in) x 0.2836 x 144 = thickness (in) x 40.84

Thickness, in (mm)Weight, lb/ft² (kg/m²)96 x 240 in plate, lb
1/4 (6.4)10.21 (49.8)1,634
5/16 (7.9)12.76 (62.3)2,042
3/8 (9.5)15.31 (74.8)2,450
1/2 (12.7)20.42 (99.7)3,267
5/8 (15.9)25.52 (124.6)4,084
3/4 (19.1)30.63 (149.5)4,901
1 (25.4)40.84 (199.4)6,534

Values are theoretical, based on nominal thickness. Actual weight varies with mill tolerance, and many shipbuilding plates are ordered in metric thicknesses. For other sizes, use our steel plate weight calculator.

Cutting and edge preparation

Hull plates, brackets, floors, web frames and collars are nested and cut on CNC tables. Plasma is fast and accurate through the thicknesses that make up most hull and deck structure, while oxy-fuel takes over for heavy plate where it cuts more economically. Our comparison of plasma vs oxy-fuel cutting covers the trade-offs.

Most butt and tee joints in ship structure need beveled edges. Cutting the bevel in the same setup as the profile saves a separate edge preparation step and keeps the bevel consistent along the edge.

  • Single V or Y bevel: one beveled edge, often with a small land, for joints welded mainly from one side.
  • Double V or X bevel: both faces beveled on thick plate to reduce weld volume and balance distortion.
  • K bevel: both faces of one plate beveled for full-penetration tee joints, such as heavy bulkhead and girder connections.

Thermal cutting leaves a thin heat-affected layer on the edge. It rarely matters for ordinary grades, but quenched and tempered naval steels may carry limits on cutting practice or require edge grinding, so check the governing specification.

Tip: Ask that heat numbers be transferred to every cut part and to remnants as part of the nest. Re-establishing traceability after parts leave the table is slow and often impossible.

Forming, straightening and surface preparation

Curved shell plates are formed in plate rolls and presses, and compound curvature near the bow and stern is often shaped by line heating. Flanged brackets and knees are formed on press brakes. Cold forming limits and minimum bend radii depend on grade and thickness, and heavy cold forming of some grades can require testing or heat treatment under class rules.

Welding heat pulls panels out of plane, so yards straighten them with heat or mechanically. Heat must stay within limits: AWS D1.1, for example, caps the temperature of areas heated for straightening at 1,100 F (600 C) for quenched and tempered steels and 1,200 F (650 C) for other steels, and naval and class rules set their own limits.

Before fabrication, plate is typically blast cleaned and coated with a thin weldable shop primer that protects it in the yard without stopping welding. Ballast tanks on many commercial ships must meet the IMO Performance Standard for Protective Coatings, which makes surface preparation and documentation part of the plate’s journey from the start.

Plate processing from ASA

American Steel & Aluminum provides heavy plate processing for defense and shipbuilding customers, with CNC plasma and oxy-fuel cutting of carbon steel up to 8 in thick and stainless up to 1.00 in, tables up to 10 x 24 ft, 5-axis bevel cutting of holes and edges and ProNest nesting. Our Saco, ME heavy plate and structural shop and our West Bath, ME defense processing facility, rail served with 22-ton cranes, support yard programs with mill certifications and full material traceability. See our plate cutting capabilities.

Frequently asked questions

What is AH36 steel plate?

AH36 is a higher-strength hull structural steel to ASTM A131 or classification society rules. It has a minimum yield strength of 51 ksi (355 MPa), a tensile strength of 71 to 90 ksi (490 to 620 MPa) and Charpy impact testing at 32 F (0 C). It is one of the most widely used grades for main hull structure in commercial ships and offshore work.

What is the difference between DH36 and EH36?

Both have the same strength: a 51 ksi (355 MPa) minimum yield. The difference is toughness testing. DH36 is impact tested at minus 4 F (minus 20 C) and EH36 at minus 40 F (minus 40 C). EH36 is assigned where structure must stay tough at lower temperatures or in critical, highly stressed locations, and it generally costs more.

Is ASTM A131 the same as ABS grade steel?

The grade designations and requirements are closely aligned, but they are not the same document. ASTM A131 is a material standard, while ABS grades are defined by ABS rules and produced under ABS survey at approved mills. A classed vessel normally needs plate certified by the classification society, so A131 material without class certification may not be accepted.

Why is shipbuilding plate shop primed?

Shop primer is a thin coating, often zinc silicate or epoxy based, applied right after blast cleaning. It protects the steel from rust while plates and parts sit in the yard through cutting, fitting and welding, and it is formulated to be welded through with limited effect on weld quality. The full paint system goes on later.

Can A36 be used instead of Grade A ship plate?

Not on a classed vessel without approval. A36 and Grade A have similar strength, but Grade A is produced and certified to ship steel rules, with controls the classification society recognizes. For unclassed boats, barges or non-structural parts, an owner or designer may accept A36, but that decision belongs to the naval architect and the vessel's rules.

Material, processing and fabrication from one supplier

Send a drawing or a material list and the ASA team will quote it from stock.